A production method for medium and thick plates for wind power towers

The method addresses surface defects and oxidation issues in wind turbine tower steel production by using shot blasting, titanium carbide-based coating, and advanced cooling and lifting techniques, resulting in high-strength, defect-free steel plates suitable for wind turbine towers.

CN115533465BActive Publication Date: 2024-12-03HEBEI PUYANG IRON & STEEL +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211398761.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-09
Publication Date
2024-12-03
Estimated Expiration
2042-11-09

AI Technical Summary

Technical Problem

Existing methods for producing medium and thick plates for wind turbine towers face challenges such as surface defects, scratches, and hooks due to fluctuating gas composition and air-fuel ratios, offline cooling causing oxidation, and inefficient lifting processes, which affect the strength, toughness, and corrosion resistance of the steel.

Method used

A method involving shot blasting, titanium carbide-based tungsten carbide coating, multi-directional descaling, online slow cooling, and flexible lifting processes to produce defect-free steel plates with high strength and toughness, using continuous casting billets and advanced rolling techniques.

Benefits of technology

The method results in zero surface defects, high strength, and improved toughness and corrosion resistance, ensuring the steel plates meet the demanding requirements of wind turbine towers, particularly in low-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003934209120000091
    Figure BDA0003934209120000091
  • Figure BDA0003934209120000101
    Figure BDA0003934209120000101
Patent Text Reader

Abstract

The present invention provides a method for producing medium and thick plates for wind turbine towers, and belongs to the technical field of metal smelting. The present invention uses continuous casting billets as production raw materials, and processes billet shot blasting, billet surface coating, billet heating, rolling, pre-straightening, UFC ultra-fast cooling, slow cooling, hoisting and spraying to prepare a medium and thick plate for wind turbine towers. The present invention adopts a casting billet coating process, and uses titanium carbide-based tungsten carbide as an anti-oxidation coating, which effectively reduces burn-in while avoiding the formation of pitting and mottled defects. The present invention adopts multi-directional descaling technology to effectively avoid the occurrence of descaling blind areas in oxidation pits of steel plates. The medium and thick plates for wind turbine towers produced by the present invention have zero surface defects and high strength and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal smelting, and in particular to a method for producing medium and thick plates for wind power towers. Background Art

[0002] In terms of wind turbine technology, which is the core of the wind power industry, modern wind turbine equipment is developing towards large-scale, high reliability, light weight and high efficiency. The capacity of a single unit is also increasing, gradually developing from hundreds of kilowatts to megawatts and even multi-megawatts. In large and medium-sized wind farms, in order to obtain more wind resources throughout the year, higher towers are used to withstand greater wind forces; in addition, due to the increase in the length of the wind blades, the mass of the entire wind turbine is also increasing, which puts higher requirements on the bearing capacity of the tower. In addition to ensuring that the tower has a high strength to support the wind power system and resist external natural forces, the special requirements of the tower for steel quality are related to the regional environment. In the "Three Norths" region, which accounts for 76% of the country's wind power installed capacity, the winter temperature is low. When selecting low-alloy tower steel, it is necessary to improve low-temperature toughness to prevent the tower from being brittle at low temperatures, so as to avoid the tower from breaking and collapsing due to impact loads under low temperature conditions. In addition, the tower steel is also required to have good fatigue life and corrosion resistance, and has high requirements for the purity, grain size, surface quality, and flaw detection of steel.

[0003] At present, there are many difficulties in controlling the surface quality of medium and thick plates used in wind turbine tower production. (1) The spot problem is difficult to solve when the gas composition and air-fuel ratio fluctuate, resulting in a large number of scrapped products. (2) The steel used in wind turbine towers needs to be slowly cooled offline and frequently hoisted, which causes scratches and hooks on the edges. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention provides a method for producing medium and thick plates for wind turbine towers, which uses continuous casting billets as production raw materials, adds a shot blasting process before the medium and thick plates enter the furnace, a high temperature resistant and anti-oxidation coating process for the continuous casting billets of the medium and thick plates, a precision rolling multi-directional descaling process, an online slow cooling process for the medium and thick plates, and a flexible lifting process for the medium and thick plates, so that the medium and thick plates for wind turbine towers prepared by the method of the present invention have zero surface defects and high strength and toughness.

[0005] The present invention provides a method for producing a medium and thick plate for a wind power tower, comprising the following steps:

[0006] (1) Steel billet shot blasting: Shot blast the surface of the steel continuous casting billet for the wind turbine tower to remove the iron oxide scale on the surface of the billet;

[0007] (2) Billet surface coating: titanium carbide-based tungsten carbide is sprayed on the billet surface by plasma spraying, with a spraying thickness of 0.5-2 μm;

[0008] (3) Billet heating: Heating is performed in a step-type double-heat storage heating furnace, wherein the heating includes one-stage heating, two-stage heating, three-stage heating and soaking treatment; the heating furnace entry temperature is ≤200°C, and the furnace exit temperature is 1100±20°C;

[0009] (4) Rolling: First, a multi-directional nozzle high-pressure water descaling technology is used to remove the coating on the surface of the steel plate, and the coating material is recovered; then rough rolling is carried out, and the starting rolling temperature of the rough rolling is 1080±20°C, and the final rolling temperature of the rough rolling is 950±20°C to reduce the secondary oxidation rate after rolling; after rough rolling, a multi-directional nozzle descaling technology is used to remove the secondary oxidation layer on the surface of the steel plate, and the steel plate is immediately cooled to the starting rolling temperature of the finishing rolling, and the starting rolling temperature of the finishing rolling is 870-920°C, and the final rolling temperature of the finishing rolling is 780-810°C; ensure that the plate type pass reduction decreases from pass to pass, and avoid excessively high final rolling temperature to cause tertiary oxidation;

[0010] (5) Pre-straightening;

[0011] (6) UFC ultra-fast cooling: Using UFC ultra-fast cooling technology, the cooling temperature after rolling is 760-790℃, and the red-return temperature is 630-670℃;

[0012] (7) Slow cooling: After the steel plate is straightened, it is directly slow cooled online. The slow cooling starting temperature is ≥450°C and the slow cooling time is 36 hours. The slow cooling is carried out in an insulation box disclosed in utility model patent CN214441886U to ensure that the thermal deformation stress is released.

[0013] (8) Hoisting and marking: hoist and mark the steel plates after slow cooling; in order to prevent damage to the steel plates, a flexible hoisting process for medium and thick plates is adopted. The utility model patent CN215279800U discloses a stacking table with a buffer structure specially used for wind power steel and a modified magnetic disk hoist (using the new magnetic disk hoist for overhead crane disclosed in the utility model patent CN209922703U) to ensure that the surface of the steel plates will not be damaged during hoisting and unloading. The hydraulic device and spring of the stacking table can effectively reduce the impact force during the stacking of steel plates, realize flexible stacking, and thus avoid scratches and bumps on the surface of the steel plates. The overhead crane hoisting process uniformly adopts a magnetic hoist with a rubber protective cover on the bottom of the magnetic disk, which can avoid problems such as hooking and scooping during the lifting and unloading process, and truly realize flexible hoisting.

[0014] Preferably, the chemical composition of the blank in step (1) is C 0.09%-0.12%, Si≤0.20%, Mn1.15-1.25%, P≤0.015, S≤0.010%, Als0.010-0.030%, Ti0.030-0.045%, B0.010-0.015%, and the remainder is Fe and unavoidable impurities.

[0015] Preferably, the specifications of the blank in step (1) are: thickness*width is 250-350mm*1800-2300mm, and the length is calculated based on the length of the finished steel plate, but does not exceed 3200mm.

[0016] Preferably, the titanium carbide-based tungsten carbide in step (2) is obtained by mixing titanium carbide and tungsten carbide powders in a mass ratio of 3:2.

[0017] Preferably, in step (3), the first stage heating temperature is 1000±20°C, the second stage heating temperature is 1150±20°C, the third stage heating temperature is 1220±20°C, the soaking stage temperature is 1190±20°C, the heating time is 8-10min / cm, and the soaking stage time is 45-50min.

[0018] Preferably, the descaling in step (4) is performed by spraying water at an angle of 15° and a descaling pressure of 22 MPa.

[0019] Preferably, the total number of passes of the finishing rolling in step (4) is 6.

[0020] The role of the surface coating in step (2) is:

[0021] a. The melting points of titanium carbide and tungsten carbide are both above 1500℃, with stable chemical properties and low porosity, which can effectively prevent the steel billet from being oxidized in the oxidizing atmosphere of the heating furnace, and play the role of anti-corrosion coating. It reduces the burning loss of the steel billet and effectively avoids the generation of pitting and spots on the steel plate.

[0022] The principle is as follows: the steel billet produces three layers of iron oxide in the heating furnace, namely the surface iron oxide layer, the middle ferric oxide layer and the bottom ferrous oxide layer. The mechanism of pitting is that the iron oxide scale is not removed cleanly after the steel billet is taken out of the furnace, and it is pressed into the surface of the steel plate to form pitting defects. The formation of spots is mostly due to the fact that the bottom ferrous oxide layer is not removed cleanly and further oxidized during the finishing rolling process to form red iron oxide, causing spotting defects. These two defects will cause uneven surface of the finished steel plate after shot blasting, affecting the painting effect. The titanium carbide-based tungsten carbide coating isolates the surface of the steel billet from the oxidizing atmosphere in the heating furnace, directly avoiding the formation of pitting and spots from the source.

[0023] b. Titanium carbide and tungsten carbide are both brittle phases and can be effectively removed in the descaling process after steelmaking. Even if a small amount remains in the rolling process, it will be crushed and the thickness is very small so as not to affect the surface quality of the steel plate.

[0024] There are scale pits formed by scale on the steel plate. The prior art uses one-way descaling, which will result in a blind area for descaling, resulting in incomplete removal of some scale. The present invention uses multi-directional descaling, eliminates the blind area for descaling, and uses opposite 15° water spraying for descaling with a descaling pressure of 22MPa, which can effectively avoid the problem of incomplete descaling.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The present invention provides a method for producing medium and thick plates for wind power towers, which has the following advantages:

[0027] 1. The casting coating process is adopted, and titanium carbide-based tungsten carbide is used as the anti-oxidation coating, which effectively reduces the burning loss and avoids the formation of pitting and mottled defects.

[0028] 2. Multi-directional descaling technology is used for descaling, which effectively avoids the descaling blind spots in the oxidation pits of the steel plate.

[0029] 3. Use online slow cooling technology to avoid various bumps and scratches caused by multiple lifting.

[0030] 4. Independently design the pallet platform and transform the magnetic lifter to achieve flexible lifting.

[0031] 5. The production method of the medium and thick plates for wind power towers of the present invention has zero surface defects and high strength and toughness. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with the embodiments.

[0033] Example 1

[0034] A method for producing medium and thick plates for wind power towers, comprising the following steps:

[0035] (1) Steel billet shot blasting: A steel continuous casting billet for wind turbine tower with a thickness and width of 350 mm and 2300 mm is selected, and the billet surface is shot blasted to remove the iron oxide scale on the billet surface; the chemical composition of the billet is C0.09%, Si0.18%, Mn1.25%, P0.011%, S0.008%, Als0.012, Ti0.045%, B0.015%, and the balance is Fe and unavoidable impurities;

[0036] (2) Billet surface coating: titanium carbide-based tungsten carbide is sprayed on the billet surface by plasma spraying, with a spraying thickness of 1.8 μm; the titanium carbide-based tungsten carbide is obtained by mixing titanium carbide and tungsten carbide powders in a mass ratio of 3:2;

[0037] (3) Billet heating: Heating is performed in a walking beam double heat storage heating furnace, wherein the heating includes first stage heating, second stage heating, third stage heating and soaking treatment; the heating furnace entry temperature is 35°C, and the furnace exit temperature is 1115°C; the first stage heating temperature is 1015°C, the second stage heating temperature is 1163°C, the third stage heating temperature is 1236°C, the soaking stage temperature is 1203°C, the heating time is 9 min / cm, and the soaking stage time is 50 min;

[0038] (4) Rolling: First, a multi-directional nozzle high-pressure water descaling technology is used to remove the coating on the surface of the steel plate, and the coating material is recovered; then rough rolling is carried out, with the starting rolling temperature of the rough rolling being 1095°C and the final rolling temperature of the rough rolling being 950°C; after rough rolling, a multi-directional nozzle descaling technology is used to remove the secondary oxide layer on the surface of the steel plate, and the steel plate is immediately cooled to the starting rolling temperature of the finishing rolling, with the starting rolling temperature of the finishing rolling being 918°C and the final rolling temperature of the finishing rolling being 803°C; the plate type pass reduction is ensured to decrease pass by pass, and the final rolling temperature is prevented from being too high to cause tertiary oxidation; the descaling is carried out by spraying water at 15° in opposite directions, and the descaling pressure is 22MPa; the total number of finishing rolling passes is 6;

[0039] (5) Pre-straightening: Use a 9-roller straightening machine for online pre-straightening, and the straightening force is not higher than 1000t.

[0040] (6) UFC ultra-fast cooling: Using UFC ultra-fast cooling technology, the cooling temperature after rolling is 788°C and the red-return temperature is 665°C;

[0041] (7) Slow cooling: After the steel plate is straightened again, it is directly slow cooled online, with the slow cooling starting temperature at 480°C and the slow cooling time at 36 hours. The slow cooling is carried out in an insulation box disclosed in utility model patent CN214441886U to ensure that the thermal deformation stress is released;

[0042] (8) Hoisting and marking: The steel plates after slow cooling are hoisted and marked; in order to prevent damage to the steel plates, a flexible hoisting process for medium and thick plates is adopted. The utility model patent CN215279800U discloses a stacking table with a buffer structure for wind power steel and a modified magnetic disk hoist (using the new type of magnetic disk hoist for overhead crane disclosed in the utility model patent CN209922703U) to ensure that the surface of the steel plates will not be damaged during hoisting and unloading. The hydraulic device and spring of the stacking table can effectively reduce the impact force during the stacking of steel plates, realize flexible stacking, and thus avoid scratches and bumps on the surface of the steel plates. The overhead crane hoisting process uniformly adopts a magnetic hoist with a rubber protective cover on the bottom of the magnetic disk, which can avoid hooking and scooping during the lifting and unloading process, and truly realize flexible hoisting; the finished thickness of the medium and thick plates is 20mm.

[0043] Example 2

[0044] A method for producing medium and thick plates for wind power towers, comprising the following steps:

[0045] (1) Steel billet shot blasting: A steel continuous casting billet for wind turbine tower with a thickness and width of 250 mm and 2300 mm is selected, and the billet surface is shot blasted to remove the iron oxide scale on the billet surface; the chemical composition of the billet is C0.08%, Si0.10%, Mn1.16%, P0.006%, S0.003%, Als0.028, Ti0.031%, B0.011%, and the balance is Fe and unavoidable impurities;

[0046] (2) Steel billet surface coating: titanium carbide-based tungsten carbide is sprayed on the steel billet surface by plasma spraying, with a spraying thickness of 0.6 μm; the titanium carbide-based tungsten carbide is obtained by mixing titanium carbide and tungsten carbide powders in a mass ratio of 3:2;

[0047] (3) Billet heating: Heating is performed in a walking beam double heat storage heating furnace, wherein the heating includes first stage heating, second stage heating, third stage heating and soaking treatment; the heating furnace entry temperature is 28°C, and the furnace exit temperature is 1118°C; the first stage heating temperature is 982°C, the second stage heating temperature is 1130°C, the third stage heating temperature is 1201°C, the soaking stage temperature is 1175°C, the heating time is 10 min / cm, and the soaking stage time is 45 min;

[0048] (4) Rolling: First, a multi-directional nozzle high-pressure water descaling technology is used to remove the coating on the surface of the steel plate, and the coating material is recovered; then rough rolling is carried out, with the starting rolling temperature of the rough rolling being 1098°C and the final rolling temperature of the rough rolling being 932°C; after rough rolling, a multi-directional nozzle descaling technology is used to remove the secondary oxide layer on the surface of the steel plate, and the steel plate is immediately cooled to the starting rolling temperature of the finishing rolling, with the starting rolling temperature of the finishing rolling being 915°C and the final rolling temperature of the finishing rolling being 782°C; the plate type pass reduction is ensured to decrease pass by pass, and the final rolling temperature is prevented from being too high to cause tertiary oxidation; the descaling is carried out by spraying water at 15° in opposite directions, and the descaling pressure is 22MPa; the total number of passes of the finishing rolling is 6;

[0049] (5) Pre-straightening: Use a 9-roller straightening machine for online pre-straightening, and the straightening force is not higher than 1000t.

[0050] (6) UFC ultra-fast cooling: Using UFC ultra-fast cooling technology, the cooling temperature after rolling is 788°C and the red-return temperature is 665°C;

[0051] (7) Slow cooling: After the steel plate is straightened again, it is directly slow cooled online, with the slow cooling starting temperature at 480°C and the slow cooling time at 36 hours. The slow cooling is carried out in an insulation box disclosed in utility model patent CN214441886U to ensure that the thermal deformation stress is released;

[0052] (8) Lifting and marking: Same as in Example 1; the finished thickness of the medium and thick plate is 8 mm.

[0053] Example 3

[0054] A method for producing medium and thick plates for wind power towers, comprising the following steps:

[0055] (1) Shot blasting of steel billet: A continuous casting billet of steel for wind turbine tower with a thickness and width of 350 mm and 2300 mm is selected, and the surface of the billet is shot blasted to remove the iron oxide scale on the surface of the billet; the chemical composition of the billet is C0.10%, Si0.18%, Mn1.20%, P0.012%, S0.008%, Als0.012, Ti0.040%, B0.015%, and the balance is Fe and unavoidable impurities;

[0056] (2) Steel billet surface coating: titanium carbide-based tungsten carbide is sprayed on the steel billet surface by plasma spraying, with a spraying thickness of 2 μm; the titanium carbide-based tungsten carbide is obtained by mixing titanium carbide and tungsten carbide powders in a mass ratio of 3:2;

[0057] (3) Billet heating: Heating is performed in a step-type double heat storage heating furnace, wherein the heating includes one-stage heating, two-stage heating, three-stage heating and soaking treatment; the heating furnace entry temperature is 100°C, and the furnace exit temperature is 1108°C; the one-stage heating temperature is 1015°C, the two-stage heating temperature is 1157°C, the three-stage heating temperature is 1232°C, the soaking section temperature is 1197°C, the heating time is 9 min / cm, and the soaking section time is 50 min;

[0058] (4) Rolling: First, a multi-directional nozzle high-pressure water descaling technology is used to remove the coating on the surface of the steel plate, and the coating material is recovered; then rough rolling is carried out, with the starting rolling temperature of the rough rolling being 1085°C and the final rolling temperature of the rough rolling being 955°C; after rough rolling, a multi-directional nozzle descaling technology is used to remove the secondary oxide layer on the surface of the steel plate, and the steel plate is immediately cooled to the starting rolling temperature of the finishing rolling, which is 910°C and the final rolling temperature of the finishing rolling is 800°C; the plate type pass reduction is ensured to decrease pass by pass, and the final rolling temperature is prevented from being too high to cause tertiary oxidation; the descaling is carried out by spraying water at 15° in opposite directions, and the descaling pressure is 22MPa; the total number of finishing rolling passes is 6;

[0059] (5) Pre-straightening: Use a 9-roller straightening machine for online pre-straightening, and the straightening force is not higher than 1000t.

[0060] (6) UFC ultra-fast cooling: Using UFC ultra-fast cooling technology, the cooling temperature after rolling is 780℃ and the red-return temperature is 650℃;

[0061] (7) Slow cooling: After the steel plate is straightened again, it is directly slow cooled online, with the slow cooling starting temperature at 480°C and the slow cooling time at 36 hours. The slow cooling is carried out in an insulation box disclosed in utility model patent CN214441886U to ensure that the thermal deformation stress is released;

[0062] (8) Lifting and marking: Same as in Example 1; the finished thickness of the medium and thick plate is 40 mm.

[0063] Example 4

[0064] A method for producing medium and thick plates for wind power towers, comprising the following steps:

[0065] (1) Steel billet shot blasting: A steel continuous casting billet for wind turbine tower with a thickness and width of 300 mm and 2300 mm is selected, and the billet surface is shot blasted to remove the iron oxide scale on the billet surface; the chemical composition of the billet is C0.11%, Si0.15%, Mn1.25%, P0.011%, S0.008%, Als0.015, Ti0.038%, B0.010%, and the balance is Fe and unavoidable impurities;

[0066] (2) Steel billet surface coating: Spray titanium carbide-based tungsten carbide on the steel billet surface by plasma spraying, with a spraying thickness of 1 μm; the titanium carbide-based tungsten carbide is obtained by mixing titanium carbide and tungsten carbide powders in a mass ratio of 3:2;

[0067] (3) Billet heating: Heating is performed in a step-beam double heat storage heating furnace, wherein the heating includes first stage heating, second stage heating, third stage heating and soaking treatment; the heating temperature entering the furnace is 75°C, and the temperature leaving the furnace is 1115°C; the first stage heating temperature is 1020°C, the second stage heating temperature is 1170°C, the third stage heating temperature is 1230°C, the soaking stage temperature is 1210°C, the heating time is 10 min / cm, and the soaking stage time is 48 min;

[0068] (4) Rolling: First, a multi-directional nozzle high-pressure water descaling technology is used to remove the coating on the surface of the steel plate, and the coating material is recovered; then rough rolling is carried out, with the starting rolling temperature of the rough rolling being 1090°C and the final rolling temperature of the rough rolling being 950°C; after rough rolling, a multi-directional nozzle descaling technology is used to remove the secondary oxide layer on the surface of the steel plate, and the steel plate is immediately cooled to the starting rolling temperature of the finishing rolling, the starting rolling temperature of the finishing rolling being 907°C, and the final rolling temperature of the finishing rolling being 800°C; the plate type pass reduction is ensured to decrease pass by pass, and the final rolling temperature is prevented from being too high to cause tertiary oxidation; the descaling is carried out by spraying water at 15° in opposite directions, and the descaling pressure is 22MPa; the total number of finishing rolling passes is 6;

[0069] (5) Pre-straightening: Use a 9-roller straightening machine for online pre-straightening, and the straightening force is not higher than 1000t.

[0070] (6) UFC ultra-fast cooling: Using UFC ultra-fast cooling technology, the cooling temperature after rolling is 775℃ and the red-return temperature is 655℃;

[0071] (7) Slow cooling: After the steel plate is straightened again, it is directly slow cooled online, with the slow cooling starting temperature at 480°C and the slow cooling time at 36 hours. The slow cooling is carried out in an insulation box disclosed in utility model patent CN214441886U to ensure that the thermal deformation stress is released;

[0072] (8) Lifting and marking: Same as in Example 1; the finished thickness of the medium and thick plate is 50 mm.

[0073] The performance test results of the medium and thick plates prepared in Examples 1-4 are shown in Table 1 with reference to GB / T1591-2018:

[0074] Table 1

[0075]

[0076]

[0077] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for producing medium and thick plates for wind power towers, characterized in that: The following steps are involved: (1) Steel billet shot blasting: Shot blast the surface of the steel continuous casting billet for the wind turbine tower to remove the iron oxide scale on the surface of the billet; (2) Billet surface coating: titanium carbide-based tungsten carbide is sprayed on the billet surface by plasma spraying, with a spraying thickness of 0.5-2 μm; (3) Billet heating: Heating is performed in a step-type double-heat storage heating furnace, wherein the heating includes one-stage heating, two-stage heating, three-stage heating and soaking treatment; the heating furnace entry temperature is ≤200°C, and the furnace exit temperature is 1100±20°C; (4) Rolling: Use multi-directional nozzle high-pressure water descaling technology to remove the coating on the steel plate, and recycle the coating material; then carry out rough rolling, the starting rolling temperature of rough rolling is 1080±20°C, and the final rolling temperature of rough rolling is 950±20°C; after rough rolling, use multi-directional nozzle descaling technology to remove the secondary oxide layer on the surface of the steel plate, and immediately enter the cooling manifold to cool to the starting rolling temperature of finishing rolling, the starting rolling temperature of finishing rolling is 870-920°C, and the final rolling temperature of finishing rolling is 780-810°C; (5) Pre-straightening; (6) UFC ultra-fast cooling: UFC ultra-fast cooling technology is used for cooling. The cooling temperature after rolling is 760-790°C, and the red-return temperature is 630-670°C. (7) Slow cooling: After the steel plate is straightened again, it is directly slow cooled online. The slow cooling starting temperature is ≥450°C and the slow cooling time is 36 hours. (8) Hoisting and marking: Hoist and mark the steel plate after slow cooling.

2. The method for producing medium and thick plates for wind power towers according to claim 1, characterized in that: The chemical composition of the blank in step (1) is: C 0.09%-0.12%, Si≤0.20%, Mn 1.15-1.25%, P≤0.015%, S≤0.010%, Als 0.010-0.030%, Ti 0.030-0.045%, B 0.010-0.015%, and the balance is Fe and unavoidable impurities.

3. The method for producing medium and thick plates for wind power towers according to claim 1, characterized in that: The specifications of the blank in step (1) are: thickness*width: 250-350mm*1800-2300mm.

4. The method for producing medium and thick plates for wind power towers according to claim 1, characterized in that: The titanium carbide-based tungsten carbide in step (2) is obtained by mixing titanium carbide and tungsten carbide powder in a mass ratio of 3:

2.

5. The method for producing medium and thick plates for wind power towers according to claim 1, characterized in that: In step (3), the first stage heating temperature is 1000±20°C, the second stage heating temperature is 1150±20°C, the third stage heating temperature is 1220±20°C, the soaking stage temperature is 1190±20°C, the heating time is 8-10min / cm, and the soaking stage time is 45-50min.

6. The method for producing medium and thick plates for wind power towers according to claim 1, characterized in that: The descaling in step (4) is performed by spraying water at an angle of 15° and a descaling pressure of 22 MPa.

7. The method for producing medium and thick plates for wind power towers according to claim 1, characterized in that: The total number of passes of the finishing rolling in step (4) is 6.