High-efficiency oil-absorbing felt and preparation method thereof

Through the graft modification and hydrophobic modification technology of polypropylene resin and polyolefin elastomer, a high-efficiency oil-absorbing felt is prepared, which solves the problems of slow oil absorption speed and low oil absorption rate at low temperature, and achieves efficient oil absorption and convenient recycling.

CN115534448BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110731465.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-29
Publication Date
2024-10-01
Estimated Expiration
2041-06-29

AI Technical Summary

Technical Problem

The existing polypropylene fiber oil-absorbing felt absorbs oil slowly under low temperature conditions, has a low oil absorption rate, and is prone to secondary leakage problems.

Method used

Polypropylene resin and polyolefin elastomer are graft-modified and then blended with polymethylmethacrylate. The inner layer is prepared through a melt-blown process, and a hydrophobic modifier is added to the outer layer to form a highly efficient oil-absorbing felt.

Benefits of technology

It increases the oil absorption rate and oil absorption ratio, enhances the low-temperature oil absorption performance and oil retention capacity, ensures the oil-water separation effect, and facilitates the recovery of oil spills.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003139373360000081
    Figure BDA0003139373360000081
  • Figure HDA0003139373370000011
    Figure HDA0003139373370000011
Patent Text Reader

Abstract

The present invention relates to a high-efficiency oil-absorbing felt and a preparation method thereof, and belongs to the technical field of polymer materials. The high-efficiency oil-absorbing felt of the present invention comprises an inner layer and an outer layer, wherein the inner layer is an oil-absorbing and oil-retaining fiber layer, which is made by blending and modifying polypropylene resin and polyolefin elastomer with polymethyl methacrylate after grafting modification, and then undergoing a melt-blowing process; the outer layer is made by melt-blowing a hydrophobically modified polypropylene resin. The high-efficiency oil-absorbing felt of the present invention has a fast oil absorption rate and a large oil retention capacity, and can be used to deal with various oil spill problems; at the same time, the present invention provides a simple and convenient preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-efficiency oil-absorbing felt and a preparation method thereof, belonging to the technical field of polymer materials. Background Art

[0002] With the rapid development of the world's oil industry, more than 60% of the total oil supply is transported by sea tankers, and offshore oil field production has also increased significantly. Oil spills have become a type of marine pollution with the highest frequency, the widest distribution area, and the greatest degree of harm.

[0003] At present, the main methods for dealing with marine oil spills are dispersion, coagulation, and adsorption. The dispersion method requires the use of dispersants to degrade the oil spills, so it is highly toxic and has a high risk of secondary environmental pollution. The coagulation method uses an oil gelling agent to quickly increase the viscosity of the oil, so that the floating oil forms lumps for easy recovery, but the production process is complex, the cost is high, and it is difficult to promote. The adsorption method is to use oil-absorbing materials to absorb the oil spills, which is the most commonly used treatment method. Adsorption materials include natural materials such as activated carbon, diatomaceous earth, cotton and linen, and artificial materials such as oil-absorbing resins, non-woven fabrics, and oil-absorbing felts. Among them, oil-absorbing felt has the characteristics of fast oil absorption, large adsorption capacity, and easy recovery, and is a commonly used oil spill treatment material.

[0004] Oil-absorbing felt materials must have the following characteristics: first, the oil absorption speed must be fast to avoid large-scale spread of oil spills; second, the water-oil separation effect is good, which is conducive to the recycling of oil spills; third, it is less affected by ambient temperature and can quickly absorb oil spills even in low temperature environments; fourth, it is non-toxic to avoid secondary environmental pollution.

[0005] Patent CN 109011708 A uses glycidyl methacrylate monomer grafted rice straw and thin velvet fiber as the middle layer of the oil-absorbing felt, and uses a coating outer layer mixed with polypropylene, polyimide and compatibilizer ABS-g-MAH.

[0006] Patent CN 104874232 A adds dry Enteromorpha between two layers of oil-absorbing fiber layers as a water-repellent and lipophilic material.

[0007] The oil-absorbing felt invented in patent CN 108297517 A has a three-layer structure, wherein the middle layer is ultra-fine environmentally friendly nanofibers made of natural fibers, polyester fibers and inorganic nanomaterials.

[0008] Currently, polypropylene fiber is a commonly used material for oil-absorbing felt, but it has problems such as slow oil absorption under low temperature conditions, low oil absorption rate, and easy secondary leakage. Summary of the invention

[0009] The purpose of the present invention is to provide a high-efficiency oil-absorbing felt, which has a fast oil absorption rate and a large oil retention capacity and can be used to deal with various oil spill problems; at the same time, the present invention provides a simple and convenient preparation method.

[0010] The high-efficiency oil-absorbing felt of the present invention comprises an inner layer and an outer layer, wherein the inner layer is an oil-absorbing and oil-retaining fiber layer, which is made by blending and modifying polypropylene resin and polyolefin elastomer with polymethyl methacrylate after grafting modification, and then undergoing a melt-blowing process;

[0011] The outer layer is made of hydrophobically modified polypropylene resin through a melt-blown process.

[0012] Preferably, the polypropylene resin is isotactic polypropylene, and its melt mass flow rate is 40 g / 10 min at 230° C. and 2.16 kg. More preferably, it is PP 2040 produced by Yanshan Petrochemical.

[0013] Preferably, the polyolefin elastomer is ethylene-octene copolymer, which has a melt mass flow rate of 20 g / 10 min at 190° C. and 2.16 kg and a Shore hardness of 88 A. More preferably, it is POE 8402 from Dow Chemical.

[0014] Preferably, the melt mass flow rate of polymethyl methacrylate is 19 g / 10 min at 230° C. and 3.8 kg. More preferably, PMMA CM-211 from Chi Mei Company of Taiwan is used.

[0015] Preferably, in the inner layer, the polypropylene resin accounts for 60-70wt% of the total amount of the three resins, the polyolefin elastomer accounts for 25-35wt% of the total amount of the three resins, and the polymethyl methacrylate resin accounts for 5wt% of the total amount of the three resins.

[0016] Preferably, the hydrophobic modifier is polyoxyethylene sorbitan monolaurate (Tween 20), polyoxyethylene sorbitan monopalmitate (Tween 40), polyoxyethylene sorbitan monooleate (Tween 60) or polyoxyethylene sorbitan monostearate (Tween 80).

[0017] The preparation method of the high-efficiency oil-absorbing felt is that the inner layer and the outer layer are prepared by quilting process, and the preparation method of the inner layer is as follows:

[0018] (1) Add polypropylene resin and polyolefin elastomer into a mixer, and then add benzoyl peroxide, maleic anhydride and liquid paraffin in sequence, and mix them evenly;

[0019] (2) granulating the resin mixed in step (1) by a parallel twin-screw extruder, wherein the twin-screw L / D is 48 and the granulation temperature is 200° C. to 220° C.;

[0020] (3) adding the graft-modified resin obtained in step (2) and polymethyl methacrylate into a mixer, adding tert-butyl peroxide, and mixing well;

[0021] (4) granulating the resin mixed in step (3) using a parallel twin-screw extruder, with a twin-screw L / D of 40 and a granulation temperature of 240° C. to 260° C.;

[0022] (5) The pellets obtained in step (4) are melt-blown into non-woven fabrics at a spinning temperature of 260° C. to 280° C. and a spinneret diameter of 0.15 mm;

[0023] (6) stacking multiple layers of the non-woven fabric obtained in step (5) to form an inner layer of the oil-absorbing felt, with a stacking thickness of 80 to 100 mm;

[0024] The outer layer is prepared as follows:

[0025] (1) adding a hydrophobic modifier to a polypropylene resin and mixing uniformly;

[0026] (2) the resin mixed in step (1) is granulated by a parallel twin-screw extruder, the twin-screw L / D=40, and the granulation temperature is 240°C to 260°C;

[0027] (3) The pellets obtained in step (2) are spun into non-woven fabrics by melt-blowing process, the spinning temperature is 260° C. to 280° C., and the spinneret diameter is 0.15 mm;

[0028] (4) The non-woven fabrics obtained in step (3) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 0.2 to 0.3 mm.

[0029] In the inner layer preparation step (1), preferably, the amount of benzoyl peroxide is 0.02% to 0.25%, the amount of maleic anhydride is 0.5% to 0.6%, and the amount of liquid paraffin is 0.5%, measured based on the total mass of the polypropylene resin and the polyolefin elastomer.

[0030] In the inner layer preparation step (3), preferably, the amount of tert-butyl peroxide used is 0.45% to 0.55%, measured based on the total mass of the polypropylene resin, the polyolefin elastomer and the polymethyl methacrylate.

[0031] In the outer layer preparation step (1), preferably, the amount of the hydrophobic modifier used is 0.01% of the mass of the polypropylene resin.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The present invention adopts a polyolefin elastomer with a long-chain branch structure and a polypropylene resin, and then uses a melt-blowing process to prepare an inner layer of the oil-absorbing felt after grafting modification. The elastomer with a long-chain branch structure can give the oil-absorbing felt good low-temperature oil absorption performance; the grafting modification of polypropylene and polyolefin elastomer can increase polarity, improve compatibility with polymethyl methacrylate, and improve oil absorption rate; the oil-absorbing felt produced after the three resins are modified has a large oil absorption amount and a good oil retention effect, and is less affected by the temperature; after the outer layer is hydrophobically modified, the oil-water separation of the oil-absorbing felt is guaranteed, which is convenient for the recovery of spilled oil. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION

[0035] The present invention is described in detail below by means of specific examples, but the present invention is not limited to these examples.

[0036] Example 1

[0037] A high-efficiency oil-absorbing felt comprises an inner layer and an outer layer.

[0038] Preparation method of inner layer:

[0039] (1) Add 60 kg of polypropylene resin PP 2040 and 35 kg of polyolefin elastomer POE 8402 into a mixer, and then add 18 g of benzoyl peroxide, 475 g of maleic anhydride and 475 g of liquid paraffin in sequence and mix well.

[0040] (2) The mixed resin in (1) was granulated by a parallel twin-screw extruder, with the twin-screw L / D = 48, the granulation barrel temperature being 210 ± 10 °C, and the die temperature being 220 °C.

[0041] (3) Add 57 kg of graft-modified resin and 3 kg of polymethyl methacrylate (PMMA CM-211) into a mixer, add 300 g of tert-butyl peroxide, and mix well.

[0042] (4) The mixed resin in (3) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0043] (5) The pellets obtained in (4) are melt-blown into non-woven fabrics at a spinning temperature of 270±10°C and a spinneret diameter of 0.15 mm.

[0044] (6) The non-woven fabrics prepared in (5) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 80 mm.

[0045] Preparation method of outer layer:

[0046] (1) Add 10 g of hydrophobic modifier Tween-60 to 100 kg of polypropylene resin PP 2040 and mix well.

[0047] (2) The resin mixed in (1) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0048] (3) The pellets obtained in (2) are spun into non-woven fabrics by melt-blowing process, the spinning temperature is 270±10°C, and the spinneret diameter is 0.15 mm.

[0049] (4) The non-woven fabrics prepared in (3) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 0.2 mm.

[0050] The inner and outer layers are reinforced by quilting and then rolled up to form the finished oil-absorbing felt.

[0051] Example 2

[0052] A high-efficiency oil-absorbing felt comprises an inner layer and an outer layer.

[0053] Preparation method of inner layer:

[0054] (1) Add 65 kg of polypropylene resin PP 2040 and 30 kg of polyolefin elastomer POE 8402 into a mixer, and then add 18 g of benzoyl peroxide, 475 g of maleic anhydride and 475 g of liquid paraffin in sequence and mix well.

[0055] (2) The mixed resin in (1) was granulated by a parallel twin-screw extruder, with the twin-screw L / D = 48, the granulation barrel temperature being 210 ± 10 °C, and the die temperature being 220 °C.

[0056] (3) Add 57 kg of graft-modified resin and 3 kg of polymethyl methacrylate (PMMA CM-211) into a mixer, add 300 g of tert-butyl peroxide, and mix well.

[0057] (4) The mixed resin in (3) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0058] (5) The pellets obtained in (4) are melt-blown into non-woven fabrics at a spinning temperature of 270±10°C and a spinneret diameter of 0.15 mm.

[0059] (6) The non-woven fabrics prepared in (5) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 90 mm.

[0060] Preparation method of outer layer:

[0061] (1) Add 10 g of hydrophobic modifier Tween-80 to 100 kg of polypropylene resin PP 2040 and mix well.

[0062] (2) The resin mixed in (1) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0063] (3) The pellets obtained in (2) are spun into non-woven fabrics by melt-blowing process, the spinning temperature is 270±10°C, and the spinneret diameter is 0.15 mm.

[0064] (4) The non-woven fabrics prepared in (3) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 0.3 mm.

[0065] The inner and outer layers are reinforced by quilting and then rolled up to form the finished oil-absorbing felt.

[0066] Example 3

[0067] A high-efficiency oil-absorbing felt comprises an inner layer and an outer layer.

[0068] Preparation method of inner layer:

[0069] (1) Add 70 kg of polypropylene resin PP 2040 and 25 kg of polyolefin elastomer POE 8402 into a mixer, and then add 18 g of benzoyl peroxide, 475 g of maleic anhydride and 475 g of liquid paraffin in sequence, and mix well.

[0070] (2) The mixed resin in (1) was granulated by a parallel twin-screw extruder, with the twin-screw L / D = 48, the granulation barrel temperature being 210 ± 10 °C, and the die temperature being 220 °C.

[0071] (3) Add 57 kg of graft-modified resin and 3 kg of polymethyl methacrylate (PMMA CM-211) into a mixer, add 300 g of tert-butyl peroxide, and mix well.

[0072] (4) The mixed resin in (3) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0073] (5) The pellets obtained in (4) are melt-blown into non-woven fabrics at a spinning temperature of 270±10°C and a spinneret diameter of 0.15 mm.

[0074] (6) The non-woven fabrics prepared in (5) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 100 mm.

[0075] Preparation method of outer layer:

[0076] (1) Add 10 g of hydrophobic modifier Tween-40 to 100 kg of polypropylene resin PP 2040 and mix well.

[0077] (2) The mixed resin in (1) is pelletized by a parallel twin-screw extruder, with L / D of the twin-screw being 40 and the pelletizing temperature being 250±100°C.

[0078] (3) The pellets obtained in (2) are spun into non-woven fabrics by melt-blowing process, the spinning temperature is 270±10°C, and the spinneret diameter is 0.15 mm.

[0079] (4) The non-woven fabrics prepared in (3) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 0.25 mm.

[0080] The inner and outer layers are reinforced by quilting and then rolled up to form the finished oil-absorbing felt.

[0081] Comparative Example 1

[0082] An oil-absorbing felt comprises an inner layer and an outer layer.

[0083] Preparation method of inner layer:

[0084] (1) Add 95 kg of polypropylene resin PP 2040 into a mixer, and add 18 g of benzoyl peroxide, 475 g of maleic anhydride and 475 g of liquid paraffin in sequence, and mix well.

[0085] (2) The mixed resin in (1) was granulated by a parallel twin-screw extruder, with the twin-screw L / D = 48, the granulation barrel temperature being 210 ± 10 °C, and the die temperature being 220 °C.

[0086] (3) Add 57 kg of graft-modified resin and 3 kg of polymethyl methacrylate (PMMA CM-211) into a mixer, add 300 g of tert-butyl peroxide, and mix well.

[0087] (4) The mixed resin in (3) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0088] (5) The pellets obtained in (4) are melt-blown into non-woven fabrics at a spinning temperature of 270±10°C and a spinneret diameter of 0.15 mm.

[0089] (6) The non-woven fabrics prepared in (5) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 80 mm.

[0090] Preparation method of outer layer:

[0091] (1) Add 10 g of hydrophobic modifier Tween-60 to 100 kg of polypropylene resin PP 2040 and mix well.

[0092] (2) The resin mixed in (1) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0093] (3) The pellets obtained in (2) are spun into non-woven fabrics by melt-blowing process, the spinning temperature is 270±10°C, and the spinneret diameter is 0.15 mm.

[0094] (4) The non-woven fabrics prepared in (3) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 0.2 mm.

[0095] The inner and outer layers are reinforced by quilting and then rolled up to form the finished oil-absorbing felt.

[0096] Comparative Example 2

[0097] An oil-absorbing felt comprises an inner layer and an outer layer.

[0098] Preparation method of inner layer:

[0099] (1) Add 60 kg of polypropylene resin PP 2040, 35 kg of polyolefin elastomer POE 8402 and 5 kg of polymethyl methacrylate PMMA CM-211 into a mixer, add 500 g of tert-butyl peroxide, and mix well.

[0100] (2) The resin mixed in (1) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0101] (3) The pellets obtained in (2) are spun into non-woven fabrics by melt-blowing process, the spinning temperature is 270±10°C, and the spinneret diameter is 0.15 mm.

[0102] (4) The non-woven fabrics prepared in (3) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 80 mm.

[0103] Preparation method of outer layer:

[0104] (1) Add 10 g of hydrophobic modifier Tween-60 to 100 kg of polypropylene resin PP 2040 and mix well.

[0105] (2) The resin mixed in (1) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0106] (3) The pellets obtained in (2) are spun into non-woven fabrics by melt-blowing process, the spinning temperature is 270±10°C, and the spinneret diameter is 0.15 mm.

[0107] (4) The non-woven fabrics prepared in (3) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 0.2 mm.

[0108] The inner and outer layers are reinforced by quilting and then rolled up to form the finished oil-absorbing felt.

[0109] Comparative Example 3

[0110] An oil-absorbing felt comprises an inner layer and an outer layer.

[0111] Preparation method of inner layer:

[0112] (1) Add 60 kg of polypropylene resin PP 2040 and 35 kg of polyolefin elastomer POE 8402 into a mixer, and then add 18 g of benzoyl peroxide, 475 g of maleic anhydride and 475 g of liquid paraffin in sequence and mix well.

[0113] (2) The mixed resin in (1) was granulated by a parallel twin-screw extruder, with the twin-screw L / D = 48, the granulation barrel temperature being 210 ± 10 °C, and the die temperature being 220 °C.

[0114] (3) Add 60 kg of graft-modified resin into a mixer, add 300 g of tert-butyl peroxide, and mix well.

[0115] (4) The mixed resin in (3) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0116] (5) The pellets obtained in (4) are melt-blown into non-woven fabrics at a spinning temperature of 270±10°C and a spinneret diameter of 0.15 mm.

[0117] (6) The non-woven fabrics prepared in (5) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 80 mm.

[0118] Preparation method of outer layer:

[0119] (1) Add 10 g of hydrophobic modifier Tween-60 to 100 kg of polypropylene resin PP 2040 and mix well.

[0120] (2) The resin mixed in (1) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0121] (3) The pellets obtained in (2) are spun into non-woven fabrics by melt-blowing process, the spinning temperature is 270±10°C, and the spinneret diameter is 0.15 mm.

[0122] (4) The non-woven fabrics prepared in (3) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 0.2 mm.

[0123] The inner and outer layers are reinforced by quilting and then rolled up to form the finished oil-absorbing felt.

[0124] Comparative Example 4

[0125] An oil-absorbing felt comprises an inner layer and an outer layer.

[0126] Preparation method of inner layer:

[0127] (1) Add 60 kg of polypropylene resin PP 2040 and 35 kg of polyolefin elastomer POE 8402 into a mixer, and then add 18 g of benzoyl peroxide, 475 g of maleic anhydride and 475 g of liquid paraffin in sequence and mix well.

[0128] (2) The mixed resin in (1) was granulated by a parallel twin-screw extruder, with the twin-screw L / D = 48, the granulation barrel temperature being 210 ± 10 °C, and the die temperature being 220 °C.

[0129] (3) Add 57 kg of graft-modified resin and 3 kg of polymethyl methacrylate (PMMA CM-211) into a mixer, add 300 g of tert-butyl peroxide, and mix well.

[0130] (4) The mixed resin in (3) is granulated by a parallel twin-screw extruder, with the twin-screw L / D = 40 and the granulation temperature being 250 ± 10 °C.

[0131] (5) The pellets obtained in (4) are melt-blown into non-woven fabrics at a spinning temperature of 270±10°C and a spinneret diameter of 0.15 mm.

[0132] (6) The non-woven fabrics prepared in (5) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 80 mm.

[0133] Preparation method of outer layer:

[0134] (1) The polypropylene resin PP 2040 is pelletized by a parallel twin screw extruder, the twin screw L / D is 40, and the pelletizing temperature is 250±10°C.

[0135] (2) The pellets obtained in (1) were melt-blown into non-woven fabrics at a spinning temperature of 270±10°C and a spinneret diameter of 0.15 mm.

[0136] (3) The non-woven fabrics prepared in (2) are stacked in multiple layers to form an inner layer of the oil-absorbing felt, with a stacking thickness of 0.2 mm.

[0137] The inner and outer layers are reinforced by quilting and then rolled up to form the finished oil-absorbing felt.

[0138] Compared with the embodiments, comparative example 1 does not add polyolefin elastomer POE 8402 resin, resulting in a lower low-temperature oil absorption rate of the oil-absorbing felt; comparative example 2 polypropylene and polyolefin elastomer resin have not been grafted and modified, and comparative example 3 does not add polymethyl methacrylate, both of which result in lower oil retention of the oil-absorbing felt; comparative example 4 has no hydrophobic modification on the outer layer, resulting in a higher water absorption of the oil-absorbing felt.

[0139] Performance Test:

[0140] The oil absorption capacity and other properties of the oil absorbent felt are tested in accordance with the requirements of JT / T 560-2004 "Marine Oil Absorbent Felt" standard.

[0141] Table 1 Oil-absorbing felt performance test results

[0142]

Claims

1. A high-efficiency oil-absorbing felt, comprising an inner layer and an outer layer, characterized in that: The inner layer and the outer layer are made by quilting technology, wherein: The preparation method of the inner layer is as follows: (1) adding polypropylene resin and polyolefin elastomer into a mixer, and then sequentially adding benzoyl peroxide, maleic anhydride and liquid paraffin, and mixing; (2) granulating the resin mixed in step (1) by a parallel twin-screw extruder, wherein the twin-screw L / D is 48 and the granulation temperature is 200° C. to 220° C.; (3) adding the graft-modified resin obtained in step (2) and polymethyl methacrylate into a mixer, adding tert-butyl peroxide, and mixing; (4) granulating the resin mixed in step (3) using a parallel twin-screw extruder, with a twin-screw L / D of 40 and a granulation temperature of 240° C. to 260° C.; (5) The pellets obtained in step (4) are melt-blown into non-woven fabrics at a spinning temperature of 260° C. to 280° C. and a spinneret diameter of 0.15 mm; (6) stacking multiple layers of the non-woven fabric obtained in step (5) to form an inner layer of the oil-absorbing felt, with a stacking thickness of 80 to 100 mm; The outer layer is prepared as follows: (1) adding a hydrophobic modifier to a polypropylene resin and mixing; (2) the resin mixed in step (1) is granulated by a parallel twin-screw extruder, the twin-screw L / D=40, and the granulation temperature is 240°C to 260°C; (3) The pellets obtained in step (2) are spun into non-woven fabrics by melt-blowing process, the spinning temperature is 260° C. to 280° C., and the spinneret diameter is 0.15 mm; (4) stacking the non-woven fabrics obtained in step (3) into an inner layer of the oil-absorbing felt in multiple layers, with a stacking thickness of 0.2 to 0.3 mm; The polyolefin elastomer is an ethylene-octene copolymer, which has a melt mass flow rate of 20 g / 10 min at 190° C. and 2.16 kg and a Shore hardness of 88A; The melt mass flow rate of the polymethyl methacrylate is 19 g / 10 min at 230° C. and 3.8 kg. The hydrophobic modifier is polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monooleate or polyoxyethylene sorbitan monostearate.

2. The high-efficiency oil-absorbing felt according to claim 1 is characterized in that: The polypropylene resin is isotactic polypropylene, and its melt mass flow rate is 40 g / 10 min at 230° C. and 2.16 kg.

3. The high-efficiency oil-absorbing felt according to claim 1 is characterized in that: In the inner layer, the polypropylene resin accounts for 60-70wt% of the total amount of the three resins, the polyolefin elastomer accounts for 25-35wt% of the total amount of the three resins, and the polymethyl methacrylate resin accounts for 5wt% of the total amount of the three resins.

4. The high-efficiency oil-absorbing felt according to claim 1 is characterized in that: In the inner layer preparation step (1), the amount of benzoyl peroxide used is 0.02% to 0.25%, the amount of maleic anhydride used is 0.5% to 0.6%, and the amount of liquid paraffin used is 0.5%, measured based on the total mass of the polypropylene resin and the polyolefin elastomer.

5. The high-efficiency oil-absorbing felt according to claim 1 is characterized in that: In the inner layer preparation step (3), the amount of tert-butyl peroxide used is 0.45% to 0.55%, measured based on the total mass of the polypropylene resin, the polyolefin elastomer and the polymethyl methacrylate.

6. The high-efficiency oil-absorbing felt according to claim 1 is characterized in that: In the outer layer preparation step (1), the amount of the hydrophobic modifier used is 0.01% of the mass of the polypropylene resin.