By combining the terminally blocked brominated epoxy resin with specific molecular weight and uncapped brominated epoxy resin, combined with glass fiber and additives, the balance of the fluidity and heat resistance of the flame retardant PBT composition is solved, and the problem of the balance of the fluidity and heat resistance of the flame retardant PBT composition is achieved. High heat resistance, high flowability and good processing performance, suitable for electronic components and other fields.

CN115536994BActive Publication Date: 2024-11-19KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211235036.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-10
Publication Date
2024-11-19
Estimated Expiration
2042-10-10

AI Technical Summary

Technical Problem

When the existing flame retardant PBT compositions improve fluidity, they tend to cause a decrease in heat resistance and fluidity regulation is difficult to achieve, which affects their processing performance during injection molding.

Method used

Using a composite of end-brominated brominated epoxy resin of specific molecular weight and unbrominated brominated epoxy resin, combined with glass fiber and other additives, the flowability and heat resistance of the flame retardant PBT composition are regulated, and the combination is adjusted by adjusting the composite The proportion achieves a balance between fluidity and heat resistance.

Benefits of technology

A flame retardant PBT composition with high heat resistance and high flowability is achieved. The flame retardant grade reaches V-0, T1% is not less than 347°C, and the melt flow rate is within the optimal range, ensuring the mechanical properties and processing of the material. Performance avoids casting and flashing phenomena.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003883318610000021
    Figure BDA0003883318610000021
  • Figure BDA0003883318610000061
    Figure BDA0003883318610000061
  • Figure BDA0003883318610000062
    Figure BDA0003883318610000062
Patent Text Reader

Abstract

The invention discloses a flame retardant PBT composition with high heat resistance and high fluidity. The flame retardant PBT composition comprises the following components calculated by weight: 40-60 parts of polybutylene terephthalate; 2-5 parts of toughening agent; 8-15 parts of flame retardant; 2-3 parts of flame retardant synergist; 25-35 parts of glass fiber; 0.5-1 part of lubricant; 0.5-1 part of other auxiliary agents; the flame retardant is a blocked brominated epoxy resin and / or an unblocked brominated epoxy resin, the flame retardant is a blocked brominated epoxy resin or a mixture of a blocked brominated epoxy resin and an unblocked brominated epoxy resin, the number average molecular weight of the blocked brominated epoxy resin is 3500-15000; the mass fraction of the blocked brominated epoxy resin in the mixture of the blocked brominated epoxy resin and the unblocked brominated epoxy resin is not less than 15%. By adjusting the ratio of the blocked brominated epoxy resin to the unblocked epoxy resin, the fluidity of the flame retardant PBT composition can be controlled. At the same time, the prepared flame retardant PBT composition has good heat resistance and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of engineering plastics, and more specifically to a flame-retardant PBT composition with high heat resistance and high fluidity, and a preparation method and application thereof. Background Art

[0002] Polybutylene terephthalate (PBT), as one of the five general engineering plastics, has excellent mechanical properties, weather resistance, aging resistance, heat resistance and solvent resistance. In addition, PBT has the advantages of fast crystallization speed, short molding cycle, low water absorption and good dimensional stability, making it widely used in the fields of electronics, home appliances, motors and coil skeletons. However, for flame-retardant reinforced PBT compositions, there is usually poor heat resistance and yellowing phenomenon; injection molding is a common production method for industrial products, and the product quality is stable, the automation level is high, and the production efficiency is high, but when the fluidity of the flame-retardant PBT composition is poor, its processing performance is affected; when the fluidity of the PBT composition is too large, it is easy to produce casting phenomenon during the injection molding process and cause flashing of the product; usually when the melt flow rate is 15.0~30.0g / 10min, the composition has relatively optimal processing fluidity and is suitable for injection molding.

[0003] Prior art CN 106147153A discloses a high-fluidity, low-melting-point glass fiber reinforced flame-retardant PBT composition, which uses a low-melting-point PET resin added to a PBT resin to improve and adjust the fluidity of the flame-retardant PBT composition. However, when the low-melting-point PET is used to improve the fluidity of PBT, there will be an ester exchange reaction in the system, which will have a certain impact on the performance and heat resistance of the flame-retardant PBT composition. Therefore, the art also needs to develop a flame-retardant PBT composition with high heat resistance and high fluidity, which has both good mechanical properties and heat resistance, and the fluidity can be regulated. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects in the above-mentioned prior art and provide a flame retardant PBT composition with high heat resistance and high fluidity, wherein the composition has excellent flame retardant properties and heat resistance, and has controllable fluidity properties.

[0005] Another object of the present invention is to provide a method for preparing the flame-retardant PBT composition with high heat resistance and high fluidity.

[0006] Another object of the present invention is to provide the application of the flame-retardant PBT composition with high heat resistance and high fluidity in electronic components, household appliances, motors and coil skeletons, and new energy vehicles.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A flame retardant PBT composition with high heat resistance and high fluidity, comprising the following components calculated in parts by weight:

[0009]

[0010] The flame retardant is a blocked brominated epoxy resin or a mixture of a blocked brominated epoxy resin and an unblocked brominated epoxy resin, and the number average molecular weight of the blocked brominated epoxy resin is 3500-15000.

[0011] The present invention provides a flame-retardant PBT composition with high heat resistance and high fluidity. The flame-retardant PBT composition with high heat resistance and high fluidity uses a capped brominated epoxy resin with a specific molecular weight and / or an uncapped brominated epoxy resin as a flame retardant. The capped brominated epoxy resin with a specific molecular weight does not react with the terminal carboxyl group in polybutylene terephthalate and has a low viscosity; while the epoxy group at the end of the uncapped brominated epoxy resin reacts with the terminal carboxyl group in polybutylene terephthalate to increase the viscosity of the system and reduce the fluidity. Therefore, the flame-retardant PBT composition prepared by compounding the capped brominated epoxy resin with a specific molecular weight and the uncapped brominated epoxy resin has good heat resistance stability; at the same time, by adjusting the ratio of the capped brominated epoxy resin and the uncapped epoxy resin, the fluidity of the flame-retardant PBT composition can be controlled.

[0012] Preferably, the number average molecular weight of the blocked brominated epoxy resin is 4,000 to 10,000.

[0013] More preferably, the number average molecular weight of the blocked brominated epoxy resin is 5000-7000.

[0014] By further adjusting the amount of the blocked brominated epoxy resin in the flame retardant, the fluidity of the flame retardant PBT composition can be improved without reducing the heat resistance stability. Preferably, the blocked brominated epoxy resin in the flame retardant accounts for more than 50% of the total mass of the flame retardant.

[0015] More preferably, the flame retardant is a blocked brominated epoxy resin.

[0016] Specifically, the blocked brominated epoxy resin is a tribromophenol blocked brominated epoxy resin.

[0017] The uncapped brominated epoxy resin is one or more of F-2100, EP-25K or CR-225K.

[0018] Preferably, the intrinsic viscosity of the polybutylene terephthalate is 0.58 to 0.85 dL / g.

[0019] More preferably, the intrinsic viscosity of the polybutylene terephthalate is 0.70 to 0.85 dL / g. The intrinsic viscosity of the polybutylene terephthalate can further improve the mechanical properties and processing properties of the flame retardant PBT composition.

[0020] Preferably, the intrinsic viscosity of the polybutylene terephthalate is tested according to ISO 1628-5-2015 standard method.

[0021] Preferably, the intrinsic viscosity of the polybutylene terephthalate is measured at a temperature of 25°C.

[0022] Preferably, the toughening agent is one or more of ethylene-acrylate or ethylene-acrylate-glycidyl ester.

[0023] More preferably, the ethylene-acrylate is one or more of ethylene-methyl acrylate or ethylene-butyl acrylate.

[0024] More preferably, the ethylene-acrylate-glycidyl ester is ethylene-methyl acrylate-glycidyl methacrylate.

[0025] Preferably, the flame retardant synergist is antimony trioxide.

[0026] Preferably, the glass fibers include chopped strand A-, E-, C-, D-, S-, and R-glass fibers, and the cross-sectional shape of the glass fibers is one of circular, elliptical, and square.

[0027] More preferably, the glass fibers are chopped strand E-glass fibers.

[0028] Preferably, the diameter of the glass fiber is 9 to 17 μm. When the diameter of the glass fiber is 9 to 17 μm, the heat resistance of the prepared PBT composition is better, T1% is not less than 347°C, the flame retardant grade reaches V-0, and the melt flow rate is better, while the mechanical properties of the flame retardant PBT composition are not significantly reduced.

[0029] In the present invention, commonly used lubricants can be selected according to the prior art, including ester grease, amide lubricant, polyethylene lubricant or stearic acid lubricant. Preferably, the lubricant is an ester lubricant.

[0030] Specifically, the ester lubricant is one or more of lower alcohol esters of fatty acids, higher alcohol esters of fatty acids, polyol esters or polyethylene glycol esters.

[0031] Preferably, the other auxiliary agent is one or more of an anti-dripping agent, an antioxidant or a nucleating agent.

[0032] In the present invention, commonly used anti-dripping agents may be selected, including but not limited to at least one of SAN-coated polytetrafluoroethylene micropowder, acrylate-coated polytetrafluoroethylene micropowder or siloxane-coated polytetrafluoroethylene micropowder.

[0033] In the present invention, commonly used nucleating agents may be selected, including but not limited to at least one of metal salt nucleating agents, organic phosphate salt nucleating agents or sorbitol nucleating agents.

[0034] Specifically, the metal salt nucleating agent is one or more of sodium benzoate, sodium stearate, calcium stearate, sodium p-phenolsulfonate, calcium p-phenolsulfonate or sodium phenolate.

[0035] Specifically, the organic phosphate salt nucleating agent is 2,2'-methylenebis(4,6-di-tert-butylphenyl) sodium phosphate or / and 2,2'-methylenebis(4,6-di-tert-butylphenyl) aluminum phosphate.

[0036] Specifically, the sorbitol nucleating agent is one or more of dibenzylidene alcohol, di(p-chlorophenyl)sorbitol, p-methylbenzylidene sorbitol or di(p-ethylbenzylidene sorbitol).

[0037] In the present invention, commonly used antioxidants can be selected, including hindered phenol antioxidants, phosphite antioxidants, diphenylamine antioxidants, copper salt antioxidants or thioether antioxidants. Preferably, the antioxidant is a hindered phenol antioxidant.

[0038] Specifically, the hindered phenol antioxidant is one or more of β(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester or 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, tetrakis[β(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester or diethylene glycol bis[methyl 3(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate].

[0039] The present invention provides a method for preparing the above-mentioned flame-retardant PBT composition with high heat resistance and high fluidity, comprising the following steps:

[0040] S1. The flame retardant and the flame retardant synergist are mixed to obtain a first mixture;

[0041] S2. The polybutylene terephthalate, toughening agent, lubricant and other additives are mixed to obtain a second mixture;

[0042] S3. The first mixed material, the second mixed material and the glass fiber are melt-blended and extruded into granules to obtain a flame-retardant PBT composition.

[0043] Preferably, in step S1., the mixing speed is 700-900 rpm.

[0044] Preferably, in step S1., the mixing time is 2 to 4 minutes.

[0045] Preferably, in step S2., the mixing speed is 600-800 rpm.

[0046] Preferably, in step S2., the mixing time is 2 to 4 minutes.

[0047] Preferably, the extrusion granulation is carried out in a twin-screw extruder.

[0048] Preferably, the temperature of zone 1 of the twin-screw extruder is 200-230°C, the temperature of zone 2 is 240-260°C, the temperature of zone 3 is 235-255°C, the temperature of zone 4 is 235-255°C, the temperature of zone 5 is 235-255°C, the temperature of zone 6 is 240-260°C, the temperature of zone 7 is 240-260°C, the temperature of zone 8 is 220-240°C, the temperature of zone 9 is 220-240°C, the temperature of zone 10 is 240-260°C, and the screw speed of the twin-screw extruder is 200-450 rpm.

[0049] The present invention protects the application of the above-mentioned flame-retardant PBT composition with high heat resistance and high fluidity in electronic components (relays, connectors, capacitors, etc.), household appliances, motors and coil skeletons, new energy vehicles, etc.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] The present invention provides a flame retardant PBT composition with high heat resistance and high fluidity. The composition uses a blocked brominated epoxy resin or a mixture of a blocked brominated epoxy resin and an unblocked brominated epoxy resin as a flame retardant. The obtained flame retardant PBT composition has good heat resistance and stability. 1% Not less than 347℃(T 1% The flame retardant grade reaches V-0 and the tensile strength is not less than 125MPa. At the same time, without adding a flow modifier, the flowability of the flame retardant PBT composition can be controlled by adjusting the ratio of the end-capped brominated epoxy resin to the unend-capped epoxy resin. The melt flow rate can be controlled at 15.5-28.6g / 10min at 250°C and 2.16kg, so that it has the best processing fluidity. In the injection molding process, there will be no glue shortage due to too low fluidity, and there will be no flash on the cast and injection molded parts due to too high fluidity. DETAILED DESCRIPTION

[0052] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.

[0053] The raw materials used in the embodiments and comparative examples of the present invention are:

[0054] PBT resin 1: PBT 1200-211M, intrinsic viscosity 0.83 dL / g, Changchun Chemical (Jiangsu) Co., Ltd.;

[0055] PBT resin 2: PBT GX111, intrinsic viscosity 0.7dL / g Jiangsu Yizheng Chemical Fiber Co., Ltd.;

[0056] Toughener: ethylene-methyl acrylate-glycidyl methacrylate block copolymer, DuPont PTW;

[0057] Flame retardant:

[0058] End-capped brominated epoxy resin 1: CR-100K, molecular weight 6000, Suzhou Borida Polymer Materials Co., Ltd.;

[0059] End-capped brominated epoxy resin 2: CR-100H, molecular weight 3500, Suzhou Borida Polymer Materials Co., Ltd.;

[0060] End-capped brominated epoxy resin 3: F-3100, molecular weight 15000, Shanghai Kain Chemical Co., Ltd.;

[0061] End-capped brominated epoxy resin 4: F-3014, molecular weight 1400, Shanghai Kain Chemical Co., Ltd.;

[0062] End-capped brominated epoxy resin 5: CR-2360, molecular weight 30000-35000, Suzhou Borida Polymer Materials Co., Ltd.;

[0063] Uncapped brominated epoxy resin: F-2100, molecular weight 20,000, Shanghai Kain Chemical Co., Ltd.;

[0064] Other brominated flame retardants: brominated polyphenylene flame retardant, SAYTEX 621, Albemarle, USA;

[0065] Flame retardant synergist: antimony trioxide, Foshan Chenti Economic and Trade Co., Ltd.

[0066] Glass fiber: HMG436S-10-4.0, diameter 10 μm, Taishan Glass Fiber Co., Ltd.; Lubricant: lipid lubricant, fatty acid lipid lubricant;

[0067] Other additives: antioxidant, hindered phenol antioxidant β (3, 5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester; anti-dripping agent, polytetrafluoroethylene anti-dripping agent, lubricant, antioxidant and anti-dripping agent are all commercially available, and the parallel tests of Examples 1 to 14 and Comparative Examples 1 to 5 all use the same lubricant and other additives.

[0068] Examples 1 to 14 and Comparative Examples 1 to 5

[0069] According to the formula in Tables 1 to 2, a flame retardant PBT composition with high heat resistance and high fluidity was prepared according to the following preparation method:

[0070] S1. The flame retardant and the flame retardant synergist are placed in a high-speed mixer and mixed for 2 to 4 minutes at a speed of 700 to 900 rpm to obtain a first mixture;

[0071] S2. The polybutylene terephthalate, toughening agent, lubricant and other additives are placed in a high-speed mixer and mixed for 2 to 4 minutes at a speed of 600 to 800 rpm to obtain a second mixture;

[0072] S3. Put the first mixed material, the second mixed material and the glass fiber into a twin-screw extruder, melt-blended and extruded to granulate to obtain a flame-retardant PBT composition; the temperature of zone 1 of the twin-screw extruder is 200-230°C, the temperature of zone 2 is 240-260°C, the temperature of zone 3 is 235-255°C, the temperature of zone 4 is 235-255°C, the temperature of zone 5 is 235-255°C, the temperature of zone 6 is 240-260°C, the temperature of zone 7 is 240-260°C, the temperature of zone 8 is 220-240°C, the temperature of zone 9 is 220-240°C, the temperature of zone 10 is 240-260°C, and the screw speed of the twin-screw extruder is 200-450 rpm.

[0073] Table 1 Amount of each component in the flame retardant PBT composition of Examples 1 to 8 (parts by weight)

[0074]

[0075] Table 2 Amount of each component in the flame retardant PBT composition in Examples 9 to 14 and Comparative Examples 1 to 5 (parts by weight)

[0076]

[0077]

[0078] Performance Testing

[0079] 1. Test methods

[0080] The performance of the flame retardant PBT composition with high heat resistance and high fluidity prepared above was tested:

[0081] (1) Tensile strength test: The flame retardant PBT composition with high heat resistance and high fluidity prepared above was tested according to standard ISO527-2012;

[0082] (2) Flame retardant performance test: The flame retardant PBT composition with high heat resistance and high fluidity prepared above was tested according to the UL94-2009 vertical burning standard;

[0083] (3) Melt flow rate test: The flame retardant PBT composition with high heat resistance and high fluidity prepared above was tested according to standard ISO 1133-2011, wherein the test conditions were 250°C / 2.16kg;

[0084] (4) Heat resistance test: The flame retardant PBT composition with high heat resistance and high fluidity prepared above was subjected to thermogravimetric analysis, and the temperature (T 1% ) to indicate the heat resistance of the material, T 1% The higher the value, the better the heat resistance of the material. The flame-retardant PBT composition with high heat resistance and high fluidity prepared above was retained in a melt indexer at 290°C for 10 minutes, and the color change was observed and recorded.

[0085] 2. Test Results The performance test results of the flame retardant PBT composition with high heat resistance and high fluidity prepared by the above method are shown in Table 3.

[0086] Table 3 Performance test results of various embodiments and comparative examples

[0087]

[0088]

[0089] It can be seen from Table 3 that the flame retardant grade of the flame retardant PBT compositions prepared in various embodiments of the present invention all reaches V-0 grade, and T 1% The temperature is not less than 347℃, and it has good mechanical properties and a wide melt flow rate, making it suitable for injection molding process, and the products are not prone to flashing.

[0090] It can be seen from Examples 1 to 4 that as the amount of the blocked epoxy resin increases, the heat stability of the flame retardant PBT composition gradually increases, it can be used at higher temperatures, has a wider range during the molding extrusion process, and the melt flow rate gradually decreases.

[0091] It can be seen from Example 3 and Examples 5 to 6 that, with the increase in the amount of toughening agent used, the heat resistance stability of the flame retardant PBT composition obtained hardly changes, and the melt flow rate gradually decreases.

[0092] It can be seen from Examples 3 and 7 to 8 that, with the increase in the amount of PBT resin used, the heat resistance stability of the flame retardant PBT composition gradually decreases, and the melt flow rate gradually increases.

[0093] It can be seen from Examples 3 and 9 to 11 that when the flame retardant is compounded with a low molecular weight end-capped brominated epoxy resin and an uncapped brominated epoxy resin, the melt flow rate of the flame retardant PBT composition is 15.5 to 28.6 g / 10 min, and the heat stability of the flame retardant PBT composition is not less than T 1% Not less than 347°C, and with the increase of the amount of the blocked brominated epoxy resin in the flame retardant, the heat stability of the flame retardant PBT composition is increased, and the fluidity is further improved. When the blocked brominated epoxy resin in the flame retardant accounts for more than 50% of the total mass of the flame retardant, the heat stability of the flame retardant PBT composition is further enhanced, and the flame retardant PBT composition does not yellow at all, T 1% Not less than 350℃, suitable for wider processing temperature.

[0094] It can be seen from Comparative Example 1 that when the molecular weight of the selected end-capped brominated epoxy resin is lower than 3500, the flame retardant grade of the flame retardant PBT composition is V-2, and the flame retardant performance is poor. 1% It is only 312℃, has poor heat stability, and is prone to yellowing.

[0095] It can be seen from Comparative Example 2 that when the molecular weight of the selected blocked brominated epoxy resin is too high, the melt flow rate of the flame retardant PBT composition is only 10.2 g / 10 min, the fluidity is poor, and glue shortage and the like will occur during the injection molding process.

[0096] It can be seen from Comparative Example 3 that when uncapped brominated epoxy resin is used, the melt flow rate of the flame retardant PBT composition is 14.5 g / 10 min, which often causes serious floating fibers on the surface of the workpiece due to poor fluidity, affecting the appearance of the material and the injection molding performance; 1% The temperature is 343°C, which is worse than that of the examples, and the yellowing of the product is relatively serious.

[0097] It can be seen from Comparative Example 4 that even if the flame retardant is a mixture of blocked brominated epoxy resin and unblocked brominated epoxy resin, when the mass fraction of the blocked brominated epoxy resin is too low, the fluidity of the flame retardant PBT composition is not significantly improved and yellowing is severe.

[0098] It can be seen from Comparative Example 5 that when brominated polyphenylene flame retardant is used as the flame retardant, the mechanical properties of the flame retardant PBT composition obtained are poor and the yellowing is serious.

[0099] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A flame retardant PBT composition with high heat resistance and high fluidity, characterized in that: It is composed of the following components calculated by weight: The flame retardant is a blocked brominated epoxy resin, and the number average molecular weight of the blocked brominated epoxy resin is 5000-6000.

2. The flame-retardant PBT composition with high heat resistance and high fluidity according to claim 1, characterized in that: The intrinsic viscosity of the polybutylene terephthalate is 0.58 to 0.85 dL / g.

3. The flame retardant PBT composition with high heat resistance and high fluidity according to claim 1, characterized in that: The toughening agent is one or more of ethylene-acrylate or ethylene-acrylate-glycidyl ester.

4. The flame retardant PBT composition with high heat resistance and high fluidity according to claim 1, characterized in that: The flame retardant synergist is antimony trioxide.

5. The flame retardant PBT composition with high heat resistance and high fluidity according to claim 1, characterized in that: The lubricant is an ester lubricant.

6. The flame retardant PBT composition with high heat resistance and high fluidity according to claim 1, characterized in that: The other auxiliary agents are one or more of an anti-dripping agent, an antioxidant or a nucleating agent.

7. The method for preparing the flame-retardant PBT composition with high heat resistance and high fluidity according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. The flame retardant and the flame retardant synergist are mixed to obtain a first mixture; S2. The polybutylene terephthalate, toughening agent, lubricant and other additives are mixed to obtain a second mixture; S3. The first mixed material, the second mixed material and the glass fiber are melt-blended and extruded into granules to obtain a flame-retardant PBT composition.