SAM-APD material based on colloidal quantum dots and silicon, preparation method thereof and SAM-APD
By using SAM-APD materials based on colloidal quantum dots and silicon in infrared photodetectors, the complex and cost-effective manufacturing problems in the prior art are solved, and high-performance infrared with high operating temperature, low power consumption and low cost are achieved Detectors are suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202211326005.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-10-20
AI Technical Summary
The manufacturing process of existing infrared photodetectors is complex and costly, making it difficult to achieve large-scale production. High-performance detectors require low operating temperatures, resulting in large device size and high power consumption, which limits the development of silicon-based optoelectronics technology.
Using SAM-APD materials based on colloidal quantum dots and silicon, including stacked Si contact layer, Si multiplier layer, Si charge layer and CQD absorption layer, the multi-exciton generation and large Bohr exciton radius characteristics of CQD are used, combined with The avalanche multiplication characteristics of the Si multiplication layer enable efficient charge carrier generation and transmission, and the responsive spectral range is adjusted by easy adjustment of QD size.
Achieve high-performance infrared APD with high operating temperature, low power consumption, and low cost, providing design freedom to control electric field, multiply gain and dark current characteristics, suitable for safe communication, monitoring and infrared imaging, and easy to use with other silicon-based optoelectronics integrated.
Smart Images

Figure CN115588703B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductors, and in particular to a SAM-APD material based on colloidal quantum dots and silicon, a preparation method thereof, and a SAM-APD. Background Art
[0002] With the continuous development of photodetectors, infrared (IR) avalanche photodetectors (APDs) have attracted the attention and research of scientific researchers due to their high performance. There are more important applications in multiple optoelectronic fields, including not only traditional infrared systems, but also emerging needs such as low-light imaging, active imaging, remote monitoring and reconnaissance, and ultra-high-speed ultimate sensitivity detection and imaging applications. Traditional infrared photodetectors are all III-V materials. At present, the III-V detector technology is very mature. In addition, the production cost of colloidal quantum dots is low, and it is expected to be used in infrared optoelectronic devices. There is no relevant report yet. Colloidal quantum dots (CQD) combined with silicon integrated infrared detectors have yet to be developed and studied.
[0003] Silicon-based optoelectronic integration is the most promising direction in today's information technology. It is considered to be the key to solving the current bottleneck problem of electronic devices and has broad application prospects. At present, the performance of silicon-based infrared lasers and waveguide devices has basically reached commercial standards, but the research on infrared detection devices is still insufficient, which has become an important factor restricting the development of silicon-based optoelectronic technology. Therefore, conducting research on infrared APD devices compatible with silicon-based technology is of great significance to the development of silicon-based integrated systems and the innovation of optoelectronic devices.
[0004] Current infrared photodetectors are mainly based on epitaxially grown materials, such as III-V materials, ternary compounds, quantum wells, and type II superlattice structures. However, the manufacture of such epitaxially grown photodetectors is usually carried out under high temperature and vacuum conditions using expensive and complex processes, which have strict requirements on growth conditions and are difficult to achieve large-scale and high-quality production. Moreover, the defects caused by epitaxial growth and the lattice mismatch caused by differences in lattice constants have a great impact on the performance of the detector, and epitaxy requires adjustment of the doping concentration, the type and proportion of multiple compound elements to achieve it, and even the introduction of other chemical elements, which increases the difficulty of the preparation process. High-performance infrared detectors usually require extremely low operating temperatures and must be equipped with a cooling system to reduce the temperature of the detector, which further increases the size, cost, and power consumption of the device, limiting its development. Summary of the invention
[0005] The purpose of the present application is to provide a SAM (absorption multiplication and separation type)-APD material based on colloidal quantum dots and silicon, a preparation method thereof and a SAM-APD to solve the above problems.
[0006] To achieve the above objectives, this application adopts the following technical solutions:
[0007] A SAM-APD material based on colloidal quantum dots and silicon, comprising a stacked Si contact layer, a Si multiplication layer, a Si charge layer, a CQD absorption layer and a CQD contact layer;
[0008] The Si multiplication layer is an n-type Si semiconductor material or a Ge / Si composite material, the CQD absorption layer is a p-type CQD, and the thickness of the CQD absorption layer is less than the diffusion length of the carriers generated by it.
[0009] Preferably, the colloidal quantum dots in the CQD absorption layer and the CQD contact layer are colloidal quantum dots with large adjustable band gaps and capable of being combined with a silicon substrate.
[0010] Preferably, the colloidal quantum dots in the CQD absorption layer and the CQD contact layer include one or more of PbSe colloidal quantum dots, PbS colloidal quantum dots, HgCdTe colloidal quantum dots, and HgTe colloidal quantum dots.
[0011] Colloidal quantum dots can be selected from HgCdTe (MCT), HgTe, PbSe, PbS, etc. HgCdTe covers a wavelength range from <2μm to >15μm and is suitable for high-temperature applications. It has become one of the world's preferred high-performance detector materials; PbSe quantum dots have a larger exciton Bohr radius and a smaller material band gap, making them suitable as light absorption layer materials.
[0012] Preferably, the Si contact layer is an n-type Si semiconductor material.
[0013] Preferably, the Si charge layer is a p-type Si semiconductor material.
[0014] The present application also provides a method for preparing the SAM-APD material based on colloidal quantum dots and silicon, comprising:
[0015] preparing a Si contact layer, a Si multiplication layer and a Si charge layer;
[0016] Then, colloidal quantum dots are sequentially arranged on the surface of the Si charge layer to obtain a CQD absorption layer and a CQD contact layer.
[0017] Preferably, the preparation of the Si contact layer, the Si multiplication layer and the Si charge layer comprises:
[0018] Si is doped by ion implantation technology to obtain a heavily doped Si contact layer, an intrinsically doped Si multiplication layer and a heavily doped Si charge layer.
[0019] Preferably, the Si multiplication layer is Si or Ge / Si composite material;
[0020] The preparation method of the Ge / Si composite material comprises:
[0021] The Si substrate with unintentional doping and oxide removed is heated in a growth chamber to obtain a clean Si surface;
[0022] A Si buffer layer is grown to smooth the surface to the atomic level, followed by Ge growth and annealing.
[0023] Preferably, the temperature of the Ge growth is 180-200° C., and the temperature of the annealing is 780-800° C.;
[0024] During the Ge growth and annealing process, the heating rate is 20° C. / min.
[0025] The present application also provides a SAM-APD, the raw materials of which include the SAM-APD material based on colloidal quantum dots and silicon.
[0026] Compared with the prior art, the beneficial effects of this application include:
[0027] The SAM-APD material based on colloidal quantum dots and silicon provided in this application provides many design freedoms to control characteristics such as electric field, multiplication gain, dark current and even excess noise; among them, CQD has the advantages of efficient multi-exciton generation (MEG) and larger Bohr exciton radius, which can achieve excellent charge carrier generation and transmission in optoelectronic devices, and the CQD absorption layer determines the multiplication carriers and the wavelength to be detected, and the Si multiplication layer determines the avalanche multiplication characteristics, such as gain, dark current and excess noise factor; the photogenerated minority carriers in the CQD absorption layer should be injected into the Si multiplication layer without loss, so p-type CQD materials should be used for manufacturing. At the same time, the multiplication layer should be n-type Si, forming a PN heterojunction so that the minority carriers (electrons) generated in the absorption layer can move freely to the Si multiplication layer, while the majority carriers (holes) cannot move to the Si multiplication layer. And the thickness of the CQD absorption layer should be less than the diffusion length of the minority carriers to ensure that all photogenerated minority carriers can diffuse to the Si multiplication layer.
[0028] The SAM-APD provided in this application belongs to CQD / Si heterogeneous infrared SAM-APD; it uses colloidal quantum dot materials with three significant advantages: the first is the ability to adjust the responsive spectral range by easily adjusting the size and system of QD; the second is to improve the structure of traditional Si-based APD photodetector devices; the third is to easily achieve silicon-based integration with other silicon-based optoelectronic detectors and meet the requirements of silicon substrates; at the same time, the above characteristics enable the device to meet the needs of specific fields, such as secure communications, monitoring and infrared imaging; and the filtering function can be integrated into the photodetector unit by utilizing the characteristics of colloidal quantum dots themselves. Therefore, the organic combination of the characteristics of colloidal quantum dots and the advantages of high gain, low noise and low cost of Si is an ideal solution for realizing high-performance infrared APD, which can achieve high operating temperature, low power consumption, low cost and large-scale integration. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0030] Figure 1 Schematic diagram of the SAM-APD structure provided for this application;
[0031] Figure 2 Schematic diagram of the energy band structure of the SAM-APD provided in this application;
[0032] Figure 3 is the photoluminescence spectrum of the obtained SAM-APD sample;
[0033] Figure 4 TEM image of the obtained SAM-APD sample.
[0034] Reference numerals:
[0035] 100-Si contact layer; 200-Si multiplication layer; 300-Si charge layer; 400-CQD absorption layer; 500-CQD contact layer. DETAILED DESCRIPTION
[0036] As used herein:
[0037] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0038] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0039] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0040] In these examples, parts and percentages are by mass unless otherwise indicated.
[0041] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0042] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0043] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0044] Example 1
[0045] This embodiment provides a preparation method of PbSe CQD / Si APD, comprising the following steps:
[0046] (1) Preparation of PbSe colloidal quantum dots: PbSe colloidal quantum dots were synthesized under a Schlenk double-row vacuum system.
[0047] a. 0.892 g of PbO, 2.825 g of oleic acid and 12.823 g of 1-octadecene were placed in a three-necked flask, which was connected to a Schlenk double-row vacuum system, and the nitrogen and vacuum switches were opened three times to reduce the water oxygen content in the flask;
[0048] b. The mixed solution was heated to 150°C under a nitrogen atmosphere to completely dissolve the yellow PbO powder, and the mixed solution was further heated to 180°C;
[0049] c. Rapidly inject 6.4g of trioctylphosphine selenium solution (containing 0.64g of selenium powder), control the temperature at 145°C as the growth temperature of PbSe colloidal quantum dots, and after a period of growth, inject excess toluene to quench the reaction. These quantum dots are separated and purified by using an acetone-ethanol mixed solution, and finally dispersed in toluene;
[0050] d. At this point, the preparation of PbSe colloidal quantum dots is completed.
[0051] (2) Si is doped by ion implantation technology to obtain heavily doped n-type Si as Si contact layer 100, intrinsically doped Si as Si multiplication layer 200, and heavily doped p-type Si as Si charge layer 300.
[0052] (3) <100> The Si wafer is cleaned and dried at a speed of 4000 rpm. Secondly, according to the optimal quantum dot growth conditions obtained previously, a layer of prepared CQD is first spin-coated on the prepared Si multiplication structure as the CQD absorption layer 400 of the APD. After that, a thin CQD film is sprayed on the spin-coated CQD as the CQD contact layer 500 of the absorption area of the APD.
[0053] The schematic diagram of the obtained SAM-APD structure is shown in Figure 1 The energy band structure diagram is shown in Figure 2 shown. Figure 3 is the photoluminescence spectrum of the obtained SAM-APD sample, Figure 4 TEM image of the obtained SAM-APD sample.
[0054] Example 2
[0055] This embodiment provides a preparation method of PbSe CQD / Si APD, comprising the following steps:
[0056] (1) Preparation of PbSe colloidal quantum dots:
[0057] a. PbO (0.892 g), oleic acid (OA) (2.600 g) and 1-octadiene (ODE) (12.848 g) were mixed in a three-necked flask and heated to 170 ° C under nitrogen until the solution became clear;
[0058] b. 6.9 mL of Se-TBP (from a stock solution of 4.5 g of Se powder dissolved in 50 mL of TBP) was quickly injected into the flask, and the mixture was cooled to 140 °C for QD growth.
[0059] c. When the particles reach the desired size, the reaction is terminated by injecting toluene;
[0060] d. At this point, the preparation of PbSe colloidal quantum dots is completed.
[0061] (2) Si is doped by ion implantation technology to obtain heavily doped n-type Si as a contact layer, heavily doped p-type Si as a charge layer, and intrinsically doped Si as a multiplication layer.
[0062] (3) <100> The Si wafer was cleaned and dried at a speed of 4000 rpm. Secondly, according to the optimal quantum dot growth conditions obtained previously, a layer of prepared CQD was first spin-coated on the prepared Si multiplication structure as the absorption layer of the APD. After that, a thin layer of CQD film was sprayed on the spin-coated CQD as the contact layer of the absorption area of the APD.
[0063] Example 3
[0064] This embodiment provides a preparation method of PbS CQD / Si APD, comprising the following steps:
[0065] (1) Preparation of PbS colloidal quantum dots:
[0066] Materials: lead nitrate, thiourea, cadmium sulfate, sodium sulfide nonahydrate, ethylene glycol, triethanolamine, ethanol and toluene.
[0067] PbS CQDs were synthesized by reacting ion source materials Pb(NO3)2 and Na2S in the presence of triethanolamine (TEA) in ethylene glycol (EG) at room temperature. All syntheses were performed at room temperature without any thermal treatment.
[0068] a. Pb(NO3)2 was dissolved in a mixed solution of 4ml TEA and 20ml EG and degassed by bubbling N2 under stirring;
[0069] b. Add 2 ml of 0.1 M Na2S in EG solution dropwise to the stirred Pb(NO3)2 solution. A black colloidal solution is formed, indicating the formation of CQDs;
[0070] c. The resulting CQDs were collected by centrifugation at 9000 rpm for 5 minutes and washed with ethanol three times. The final product was dispersed in ethanol for the following measurements;
[0071] d. At this point, the preparation of PbS colloidal quantum dots is completed.
[0072] (2) Si is doped by ion implantation technology to obtain heavily doped n-type Si as a contact layer, heavily doped p-type Si as a charge layer, and intrinsically doped Si as a multiplication layer.
[0073] (3) <100> The Si wafer was cleaned and dried at a speed of 4000 rpm. Secondly, according to the optimal quantum dot growth conditions obtained previously, a layer of prepared CQD was first spin-coated on the prepared Si multiplication structure as the absorption layer of the APD. After that, a thin layer of CQD film was sprayed on the spin-coated CQD as the contact layer of the absorption area of the APD.
[0074] Example 4
[0075] This embodiment provides a method for preparing a HgCdTe CQD / Si APD, comprising the following steps:
[0076] (1) Preparation of HgCdTe colloidal quantum dots:
[0077] a. The cadmium and mercury precursors (HgCl2, CdCl2) were placed in a solvent stored in a 3-necked flask at T = 100 ° C (36 mgHgCl2 and 4 mg CdCl2 were added to 4 mL of oleylamine, and the molar ratio of Cd / Hg was maintained at ~0.11);
[0078] b. By blowing high purity gas at 100 ° C for one hour, the mixture was stirred continuously and maintained under a nitrogen environment;
[0079] c. After 1 hour, 0.1 mL of a 0.5 M tellurium (Te) precursor solution in tri-n-octylphosphine (TOP) was injected into the above mixture. A colorless solution that rapidly changed from brown to black was formed, indicating the onset of the nucleation process and further growth of the particles;
[0080] d. At this point, the preparation of HgCdTe colloidal quantum dots is completed. Here, the size of the particles is determined by the growth parameters, such as temperature, concentration and growth time.
[0081] (2) Si is doped by ion implantation technology to obtain heavily doped n-type Si as a contact layer, heavily doped p-type Si as a charge layer, and intrinsically doped Si as a multiplication layer.
[0082] (3) The measured size of CQD synthesized in 60 minutes is about 14nm. <100> After the Si wafer was cleaned and dried at 4000 rpm, HgCdTe CQDs were drop-casted on Si to achieve a uniform CQD film layer, and then a thin CQD film was sprayed as the contact layer of the absorption region of the APD.
[0083] Example 5
[0084] This embodiment provides a method for preparing a HgCdTe CQD / Si APD, comprising the following steps:
[0085] (1) Preparation of HgCdTe colloidal quantum dots:
[0086] a. The cadmium and mercury precursors (HgCl2, CdCl2) were placed in a solvent stored in a 3-necked flask at T = 120°C (36 mgHgCl2 and 4 mg CdCl2 were added to 4 mL of oleylamine, and the molar ratio of Cd / Hg was maintained at ~0.11);
[0087] b. By blowing high purity gas at 110 ° C for one hour, stirring the mixture continuously and maintaining it under nitrogen environment;
[0088] c. After 1 hour, 0.1 mL of a 0.5 M tellurium (Te) precursor solution in tri-n-octylphosphine (TOP) was injected into the above mixture. A colorless solution that rapidly changed from brown to black was formed, indicating the onset of the nucleation process and further growth of the particles;
[0089] d. At this point, the preparation of HgCdTe colloidal quantum dots is completed. Here, the size of the particles is determined by the growth parameters, such as temperature, concentration and growth time.
[0090] (2) Si is doped by ion implantation technology to obtain heavily doped n-type Si as a contact layer, heavily doped p-type Si as a charge layer, and intrinsically doped Si as a multiplication layer.
[0091] (3) The measured size of CQD synthesized in 60 minutes is about 14nm. <100> After the Si wafer was cleaned and dried at 4 000 rpm, HgCdTe CQDs were drop-casted on Si to achieve a uniform CQD film layer, and then a thin CQD film was sprayed as the contact layer of the absorption region of the APD.
[0092] Example 6
[0093] This embodiment provides a method for preparing a HgCdTe CQD / Si APD, comprising the following steps:
[0094] (1) Preparation of HgCdTe colloidal quantum dots:
[0095] a. 0.3 m thioglycolic acid (TGA) was dissolved in 115 m water and 0.537 g (2 mmol) of CdCl2·5H2O was added under stirring, and the pH value of the solution was adjusted to 12 by dropwise addition of 1 M NaOH solution;
[0096] b. After adding 1.25 g (33 mmol) of NaBH4, gradually dropwise add 10 ml of 0.1 M Na2TeO3 solution;
[0097] c. The reaction vessel was then transferred to a 95°C oil bath and heated for 1 hour to obtain a CdTe QDs precursor;
[0098] d. Dissolve 0.091 g Hg(NO3)2·H2O in 20 mL of high purity water to form a 13.3 mM Hg solution;
[0099] e. Under vigorous stirring, 0.5, 1.0 and 2.0 mL of Hg(NO3)2 solution was dropped into three prepared 15 mL CdTe QDs precursor solutions and placed at room temperature in the dark for 24 h;
[0100] f. At this point, the preparation of HgCdTe colloidal quantum dots is completed.
[0101] (2) Si is doped by ion implantation technology to obtain heavily doped n-type Si as a contact layer, heavily doped p-type Si as a charge layer, and intrinsically doped Si as a multiplication layer.
[0102] (3) The measured size of CQD synthesized in 60 minutes is about 14nm. <100> After the Si wafer was cleaned and dried at 4000 rpm, HgCdTe CQDs were drop-casted on Si to achieve a uniform CQD film layer, and then a thin CQD film was sprayed as the contact layer of the absorption region of the APD.
[0103] Example 7
[0104] This embodiment provides a method for preparing a HgTe CQD / Si APD, comprising the following steps:
[0105] (1) Preparation of HgTe colloidal quantum dots:
[0106] a. 70 mg HgCl2 was dissolved in octadecylamine (ODA), stirred and heated at 120 ° C under a vacuum of 0.2 mbar for one hour;
[0107] b. 10 mL of 80% oleylamine (OLA) was degassed under vacuum and 0.2 mL of dry 1MTOP:Te was added and stored under nitrogen until needed;
[0108] c. The Hg / ODA solution was placed under nitrogen and cooled to 60°C. At this point TOP:Te / OLA was rapidly injected and the solution was reheated to the desired temperature of 80-110°C;
[0109] d. The solution does not turn black immediately at this point, but rather progresses from light brown to black as nanocrystals (NCs) form. The solution is kept at the desired temperature for 5 minutes after injection. The growth is quenched by adding 31.5 mL tetrachloroethylene (TCE) and 3.5 mL DDT and cooling to room temperature.
[0110] e. Nanocrystal purification: The growth solution was mixed with methanol in a 1:1 ratio and centrifuged. The supernatant was removed and the process was repeated twice. After the final collision, the NCs were redispersed in chloroform at a density of 20 mg / mL. (None of the solvents used were anhydrous);
[0111] f. At this point, the preparation of HgCdTe colloidal quantum dots is completed.
[0112] (2) Si is doped by ion implantation technology to obtain heavily doped n-type Si as a contact layer, heavily doped p-type Si as a charge layer, and intrinsically doped Si as a multiplication layer.
[0113] (3) HgTe CQDs in chloroform are sprayed onto the Si multiplication structure as the absorption layer of the APD. After that, a thin CQD film is sprayed on the spin-coated CQDs as the contact layer of the absorption region of the APD.
[0114] Example 8
[0115] This embodiment provides a method for preparing a HgTe CQD / Si APD, comprising the following steps:
[0116] (1) Preparation of HgTe colloidal quantum dots:
[0117] a. Dissolve mercuric chloride (HgCl2) powder in oleylamine at 100°C under argon protection for 2 hours to obtain a transparent and clear solution. The concentration of HgCl2 / oleylamine solution is 0.1mM;
[0118] b. Telluride (Te) powder was dissolved in tri-n-octylphosphine (TOP) to produce a bright green solution with a concentration of 1 M;
[0119] c. Growth of HgTe CQDs: 0.4 mL of Te / TOP was quickly injected into a flask containing 16 mL of HgCl2 / oleylamine. HgTe nanocrystals began to grow and the mixture immediately turned black.
[0120] d. The final size of the quantum dots is determined by the reaction temperature (in the range of 80-100°C) and the reaction time (1-100 minutes). The reaction was quenched by extracting the mixture containing HgTe quantum dots into a solution of 10% dodecanethiol and 1% TOP in tetrachloroethylene. The CQDs were then purified by precipitation with ethanol and redispersion in tetrachloroethylene.
[0121] e. At this point, the preparation of HgCdTe colloidal quantum dots is completed.
[0122] (2) Si is doped by ion implantation technology to obtain heavily doped n-type Si as a contact layer, heavily doped p-type Si as a charge layer, and intrinsically doped Si as a multiplication layer.
[0123] (3) HgTe CQDs in chloroform are sprayed onto the Si multiplication structure as the absorption layer of the APD. After that, a thin CQD film is sprayed on the spin-coated CQDs as the contact layer of the absorption region of the APD.
[0124] Example 9
[0125] The difference from Example 8 is that the Si multiplication layer is replaced by Ge / Si.
[0126] Preparation method of Ge / Si:
[0127] a. An unintentionally doped Si(100) substrate (resistivity > 10000Ω·cm) was used without intentional corner cutting. Before loading into the MBE system, the Si substrate was etched by HF (8%) to remove the native oxide;
[0128] b. Transfer them to the growth chamber and heat to 700 ° C for 10 minutes to obtain a clean Si surface;
[0129] c. Grow a 40nm Si buffer layer to further smooth the surface to the atomic level. Ge growth is carried out at a lower temperature (200℃), and subsequent annealing is carried out at 800℃;
[0130] There are two reasons for choosing 200°C as the Ge growth temperature: first, the interdiffusion between Ge and Si can be suppressed at lower temperatures. Second, lower temperatures are beneficial for heteroepitaxial growth with large lattice mismatch. During the growth and annealing process, the background is kept at 10 -10mbar level. The thickness of the grown Ge film was 500 nm to obtain a fully relaxed film. For growth and annealing, the heating rate of the heater was kept at 20 °C / min to avoid possible cracking of the film due to mismatch in thermal expansion coefficients;
[0131] d. At this point, the preparation of Ge / Si is completed.
[0132] Comparative Example 1
[0133] This comparative example provides a multiplication absorption separation Si-Ge APD.
[0134] In this APD structure, the waveguide Si-Ge APD consists of a germanium absorption layer, a silicon charge layer, a silicon multiplication layer, and a silicon n-contact layer from top to bottom. A relatively low electric field is maintained in germanium, and a high electric field is maintained in silicon to achieve high GBP and low operating voltage. Light absorption and carrier multiplication occur in the Ge absorption layer and the Si multiplication layer, respectively. The Ge material with a relatively narrow bandgap in the light absorption region provides long-wavelength sensitivity, while the silicon in the multiplication region reduces the tunneling current, which can achieve low bias and low noise. However, the SiAPD response band is too single compared to the proposed SAM-APD response band based on colloidal quantum dots and Si, and cannot be used for mid-infrared band operation, and the production cost of colloidal quantum dots is lower.
[0135] preparation:
[0136] (1) After removing particles and natural oxide layer on the wafer surface through standard cleaning, device preparation officially begins.
[0137] (2) Dry etching is used to etch the single-mode waveguide, and ICP (inductively coupled plasma) etching technology is used to deeply etch the top silicon. Since the etching selectivity of Si to SiO2 exceeds 30, the buried oxide layer is used as an etching stop layer.
[0138] (3) PECVD (plasma enhanced chemical vapor deposition) is used to deposit the SiO2 layer, which plays a role in reducing injection damage and inhibiting the channel effect. After coating, exposure, and development, high-dose, low-energy P ions are injected into the heavily doped area to form a shallower heavily doped distribution. This is to reduce the impurity diffusion caused by subsequent heat treatment. The same process steps are used to inject B ions into the area. After ion implantation, the wafer is subjected to rapid thermal annealing (RTA) to repair the implantation damage and activate the implanted ions.
[0139] (4) A higher quality germanium layer can be obtained by combining low temperature buffer layer technology with selective area epitaxial growth technology.
[0140] The SAM-APD material based on colloidal quantum dots and silicon and the preparation method thereof and SAM-APD provided in this application have the following advantages:
[0141] 1. A new APD absorption layer and multiplication layer material combination is proposed, using colloidal quantum dots combined with Si or Ge / Si as the absorption layer and multiplication layer of APD. Through reasonable energy band design, it can effectively block the motion of multiple carriers, reduce dark current, and improve device performance.
[0142] 2. By using colloidal quantum dots combined with Si structure, the device can achieve high operating temperature, high gain and low noise.
[0143] 3. The use of colloidal quantum dots combined with Si structure simplifies material growth, reduces costs, and is expected to achieve large-scale integration.
[0144] 4. The spectral response range is: PbSe CQD: 1.7-2.1μm, PbS CQD: 0.8-1.7μm, HgCdTe CQD: 3-5μm, HgTe CQD: 1.1-2.6μm.
[0145] 5. The grain size of PbSe CQD is about 8nm, the grain size of PbS CQD is about 5nm, the grain size of HgCdTe CQD is about 14nm, and the grain size of HgTe CQD is about 8nm.
[0146] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0147] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A SAM-APD based on colloidal quantum dots and silicon, characterized in that: It includes a stacked Si contact layer, a Si multiplication layer, a Si charge layer, a CQD absorption layer and a CQD contact layer; The Si multiplication layer is an n-type Si semiconductor material or a Ge / Si composite material, the CQD absorption layer is a p-type CQD, and the thickness of the CQD absorption layer is less than the diffusion length of the carriers generated by it; The colloidal quantum dots in the CQD absorption layer and the CQD contact layer include one or more of PbSe colloidal quantum dots, PbS colloidal quantum dots, HgCdTe colloidal quantum dots, and HgTe colloidal quantum dots; The Si contact layer is an n-type Si semiconductor material; The Si charge layer is a p-type Si semiconductor material.
2. A method for preparing a SAM-APD based on colloidal quantum dots and silicon according to claim 1, characterized in that: include: preparing a Si contact layer, a Si multiplication layer and a Si charge layer; Then, colloidal quantum dots are sequentially arranged on the surface of the Si charge layer to obtain a CQD absorption layer and a CQD contact layer.
3. The preparation method according to claim 2, characterized in that: The preparation of the Si contact layer, the Si multiplication layer and the Si charge layer comprises: Si is doped by ion implantation technology to obtain a heavily doped Si contact layer, an intrinsically doped Si multiplication layer and a heavily doped Si charge layer.
4. The preparation method according to claim 2, characterized in that: The Si multiplication layer is Si or Ge / Si composite material; The preparation method of the Ge / Si composite material comprises: The Si substrate with unintentional doping and oxide removed is heated in a growth chamber to obtain a clean Si surface; A Si buffer layer is grown to smooth the surface to the atomic level, followed by Ge growth and annealing.
5. The preparation method according to claim 4, characterized in that: The temperature of the Ge growth is 180-200° C., and the temperature of the annealing is 780-800° C.; During the Ge growth and annealing process, the heating rate is 20° C. / min.
6. A SAM-APD, characterized in that: The raw materials include the SAM-APD based on colloidal quantum dots and silicon as claimed in claim 1.
Citation Information
Patent Citations
Avalanche photodiode
CN105637657A
Monolithic integrated ultraviolet-infrared bi-color avalanche photodiode and manufacturing method thereof
CN106847933A
PbS quantum dot Si-APD infrared detector and preparation method thereof
CN110350045A
Quantum dot wide range single -photon detector
CN206210817U
Photodetection element including photoelectric conversion structure and avalanche structure