A pultruded profile for photovoltaic module frame, a photovoltaic module frame and its manufacturing method

By introducing longitudinal and transverse reinforcing materials into the polyurethane resin substrate of the photovoltaic frame, the problem of insufficient strength of existing materials is solved, resulting in a high-strength, environmentally friendly and low-cost photovoltaic frame material suitable for fixing and protecting photovoltaic modules.

CN115625909BActive Publication Date: 2026-11-10JINKO SOLAR CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211203982.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-29
Publication Date
2026-11-10
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

Existing photovoltaic frame materials such as aluminum alloys and galvanized steel consume a lot of metal resources and are costly. Composite materials have great development potential, but existing composite materials are not strong enough, especially under pressure they are prone to longitudinal tearing.

Method used

The profile is made of polyurethane resin matrix with longitudinal and transverse reinforcement materials. The longitudinal reinforcement material is composed of interlaced glass fiber yarn, glass fiber and glass fiber mat, while the transverse reinforcement material is composed of chopped glass fiber dispersed in polyurethane resin matrix, which improves the longitudinal and transverse strength of the profile.

Benefits of technology

It significantly improves the longitudinal and lateral strength of the photovoltaic module frame, preventing longitudinal tearing under pressure, and the material is environmentally friendly and has a low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115625909B_ABST
    Figure CN115625909B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of solar cell technology and provides a pultruded profile for photovoltaic module frames, a photovoltaic module frame, and a method for its fabrication. The pultruded profile for photovoltaic module frames provided by this invention includes a polyurethane resin matrix and longitudinal and transverse reinforcing materials impregnated in the polyurethane resin matrix. The longitudinal reinforcing material includes glass fiber yarns, glass fibers, and glass fiber mats continuously extending in the longitudinal direction of the profile. At any cross-section of the profile: the glass fiber yarns are interlaced, the glass fibers are densely distributed between the glass fiber yarns, and the glass fiber mat wraps around the outer periphery of the profile cross-section. The transverse reinforcing material includes chopped glass fibers dispersed in the polyurethane resin matrix. The pultruded profile for photovoltaic module frames provided by this invention not only has high longitudinal strength but also significantly improved transverse strength, effectively preventing tearing of the frame profile along the longitudinal direction under pressure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solar cell technology, and specifically relates to a pultruded profile for photovoltaic module frames, a photovoltaic module frame, and a method for its preparation. Background Technology

[0002] Solar energy is one of the most important clean and renewable energy sources. With the development of photovoltaic technology, the cost of photovoltaic power generation has approached that of thermal power. Due to its low investment, zero pollution, long lifespan, and short investment payback period, photovoltaic power generation is becoming increasingly popular.

[0003] Solar photovoltaic (PV) modules are crucial devices for converting solar energy into electrical energy. PV frames are essential components for securing these modules, protecting them from corrosion and wind damage. The material requirements for PV frames include high strength, lightweight, aesthetic appeal, and low cost. Currently, commonly used materials for solar PV frame supports include aluminum alloy, galvanized steel, and composite materials. Aluminum alloy is the most widely used, but manufacturing aluminum alloy and galvanized steel frames requires significant metal resources, resulting in high costs. Therefore, composite material frames have enormous development potential. Summary of the Invention

[0004] The purpose of this invention is to provide a pultruded profile for photovoltaic module frames, a photovoltaic module frame, and a method for its preparation.

[0005] To address the aforementioned technical problems, a first aspect of the present invention provides a pultruded profile for a photovoltaic module frame, the profile comprising a polyurethane resin matrix and longitudinal and transverse reinforcing materials impregnated in the polyurethane resin matrix; wherein the longitudinal reinforcing material comprises glass fiber yarns, glass fibers, and glass fiber mats continuously extending in the longitudinal direction of the profile; on any cross-section of the profile: the glass fiber yarns are interlaced, the glass fibers are densely distributed between the glass fiber yarns, and the glass fiber mat is wrapped around the outer periphery of the cross-section of the profile; the transverse reinforcing material comprises chopped glass fibers dispersed in the polyurethane resin matrix.

[0006] Compared to existing technologies, this invention provides a polyurethane resin-based frame profile comprising longitudinal and transverse reinforcement materials, both of which are impregnated within a polyurethane resin matrix. The longitudinal reinforcement materials include glass fiber yarns, glass fibers, and glass fiber mats extending continuously in the longitudinal direction of the profile, all of which contribute to enhancing the longitudinal strength of the profile. At any cross-section of the profile, the glass fiber yarns are interlaced, with the glass fibers densely distributed among them, and the glass fiber mat wrapping around the outer periphery of the profile's cross-section. Because the glass fiber yarns are interlaced within the profile, tearing along the longitudinal direction of the frame profile under pressure is more effectively prevented, significantly improving the transverse strength of the profile. Furthermore, the transverse reinforcement materials include chopped glass fibers dispersed within the polyurethane resin matrix, which further enhance the transverse strength of the frame profile. Therefore, the pultruded frame profile for photovoltaic modules provided by this invention possesses both high longitudinal and transverse strength.

[0007] As a preferred embodiment, the pultruded profile for photovoltaic module frames provided by the present invention comprises, by weight: 20-30 parts of polyurethane resin matrix, 30-60 parts of glass fiber yarn, 5-25 parts of glass fiber, 5-20 parts of glass fiber mat, and 1-10 parts of chopped glass fiber.

[0008] More preferably, the pultruded profile for photovoltaic module frames provided by the present invention comprises, by weight: 20-25 parts of polyurethane resin matrix, 40-50 parts of glass fiber yarn, 10-20 parts of glass fiber, 10-14 parts of glass fiber mat, and 5-6 parts of chopped glass fiber.

[0009] More preferably, in addition to the polyurethane resin matrix, glass fiber yarn, glass fiber, glass fiber mat and chopped glass fiber mentioned above, the pultruded profile for photovoltaic module frames provided by the present invention may further include, by weight, 0.1 to 0.1 parts of antioxidant, 0.1 to 1 part of ultraviolet absorber, 0.1 to 1 part of light stabilizer, 0.1 to 1 part of water absorber, 0.1 to 1 part of wetting and dispersing agent, 0.1 to 1 part of defoamer, and 0.2 to 2 parts of release agent.

[0010] By adjusting the mass ratio of polyurethane resin matrix, glass fiber yarn, glass fiber, glass fiber mat, and chopped glass fiber to the preferred range provided by this invention, the longitudinal and transverse strengths of the frame profile can be kept within an optimal range. Furthermore, by adding antioxidants, ultraviolet absorbers, and light stabilizers to the polyurethane resin matrix, the prepared frame profile is less prone to yellowing, thus improving its mechanical properties under prolonged outdoor exposure.

[0011] Optionally, in the pultruded profile for photovoltaic module frames provided by the present invention, the polyurethane resin is a polymer of isocyanate and polyol, wherein the isocyanate is selected from at least one of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isoflurane diisocyanate and dicyclohexylmethane-4,4'-diisocyanate; and the polyol is selected from polyether polyol or polyester polyol.

[0012] Optionally, in the pultruded profile for photovoltaic module frames provided by the present invention, the antioxidant is selected from phenolic, phosphite, or ketone antioxidants; the ultraviolet absorber is selected from ketone or triazole ultraviolet absorbers; the light stabilizer is selected from ester or phosphite light stabilizers; and the water absorber is a molecular sieve water absorber.

[0013] Preferably, in the pultruded profile for photovoltaic module frames provided by the present invention, the linear density of the glass fiber yarn is 2400-4800 g / km; the diameter of the glass fiber is 10-30 μm; and the thickness of the glass fiber mat is 0.2-2 mm.

[0014] Preferably, in the pultruded profile for photovoltaic module frames provided by the present invention, the diameter of the chopped glass fibers is 10-30 μm, and the length of the chopped glass fibers is 1-5 mm; on any cross-section of the profile: the unit area distribution density F0 of the chopped glass fibers at any position and the unit area distribution density F of the chopped glass fibers at a distance of 10 cm from the position are... 10 The relative deviation (F0-F) 10 The absolute value of ) / F0 does not exceed 20%.

[0015] More preferably, in the pultruded profile for photovoltaic module frames provided by the present invention, the diameter of the chopped glass fibers is 18-25 μm, and the length of the chopped glass fibers is 2-3 mm; on any cross-section of the profile: the unit area distribution density F0 of the chopped glass fibers at any position and the unit area distribution density F0 of the chopped glass fibers at a distance of 10 cm from the position are... 10 The relative deviation (F0-F) 10 The absolute value of ) / F0 does not exceed 10%.

[0016] In this invention, when the mass fraction of chopped glass fibers in the polyurethane resin matrix is ​​within a certain range, adjusting the diameter and length of the chopped glass fibers to a preferred range can improve the uniformity of the distribution of chopped glass fibers in the polyurethane resin matrix, thereby enabling the frame profile to obtain better lateral strength.

[0017] A second aspect of the present invention provides a photovoltaic module frame, which is prepared using a pultruded profile for photovoltaic module frames provided in the first aspect of the present invention. Since the pultruded profile for photovoltaic module frames provided in the first aspect of the present invention has good longitudinal and transverse strength, the photovoltaic module frame prepared from this profile also has good longitudinal and transverse strength, and in particular, will not tear along the longitudinal direction of the profile under pressure.

[0018] Optionally, the photovoltaic module frame includes a receiving groove for mounting the photovoltaic module laminate and a support portion located below the receiving groove. The bottom of the receiving groove and the top of the support portion share a top bearing surface. The receiving groove also includes a first limiting surface and a second limiting surface, which are sequentially joined together to form the receiving groove. The receiving groove is open on one side. The support portion also includes a first side surface, a bottom bearing surface, and a second side surface, which are sequentially joined together to form a closed cavity.

[0019] Optionally, the photovoltaic module frame includes a receiving groove for mounting the photovoltaic module laminate and a support portion located below the receiving groove. The bottom of the receiving groove and the top of the support portion share a top bearing surface. The receiving groove also includes a first limiting surface and a second limiting surface, which are sequentially joined together to form the receiving groove. The receiving groove is open on one side. The support portion also includes a first side surface and a bottom bearing surface, which are sequentially joined together to form an open cavity. The opening direction of the cavity is opposite to the opening direction of the receiving groove.

[0020] A third aspect of the present invention provides a method for preparing the photovoltaic module frame described in the second aspect, comprising the following steps:

[0021] S1: The polyol, the raw material for preparing the polyurethane resin, and the additives in the profile are stirred and mixed in a mixing tank. The chopped glass fibers are added and stirring is continued to obtain a resin premix in which the chopped glass fibers are uniformly dispersed.

[0022] S2: The glass fiber yarn, the glass fiber, and the glass fiber mat are fed through a yarn feeding device, shaped through a yarn threading mold to obtain the longitudinal reinforcing material, and then guided into a resin tank through a guiding device;

[0023] S3: Mix the resin premix and the isocyanate, the raw material for preparing the polyurethane resin, in a certain proportion, and inject the mixture into the resin tank through a dispensing machine to impregnate the longitudinal reinforcing material, and then heat and pre-cur it.

[0024] S4: The pre-cured product is cured in a thermoforming mold;

[0025] S5: Pull out the pultruded profile for the photovoltaic module frame from the outlet of the heating and forming mold using a traction device, and cut it into a photovoltaic module frame suitable for the size of the photovoltaic laminate. Attached Figure Description

[0026] Figure 1 This is a schematic cross-sectional view of a pultruded profile for a photovoltaic module frame according to an embodiment of the present invention;

[0027] Figure 2 This is a process flow diagram of the fabrication process of a photovoltaic module frame according to an embodiment of the present invention;

[0028] Figure 3 This is a three-dimensional structural diagram of a photovoltaic module frame according to an embodiment of the present invention;

[0029] Figure 4 This is a three-dimensional structural diagram of a photovoltaic module frame according to another embodiment of the present invention. Detailed Implementation

[0030] To better understand the purpose, features, and advantages of this invention, the embodiments of this invention will be described in detail below with reference to the accompanying drawings.

[0031] Some embodiments of the present invention provide a pultruded profile for a photovoltaic module frame. Figure 1 This is a schematic cross-sectional view of a pultruded profile for a photovoltaic module frame according to an embodiment of the present invention. The profile includes a polyurethane resin matrix 1 and longitudinal and transverse reinforcing materials impregnated in the polyurethane resin matrix 1; wherein, the longitudinal reinforcing material includes glass fiber yarns 2, glass fibers 3, and glass fiber mats 4 extending continuously in the longitudinal direction of the profile. The longitudinal reinforcing material extends continuously in the longitudinal direction of the profile, improving the longitudinal strength of the profile. In any cross-section of the profile: the glass fiber yarns 2 are staggered and layered, the glass fibers 3 are densely distributed between the glass fiber yarns 2, and the glass fiber mats 4 are wrapped around the outer periphery of the profile cross-section. Because the glass fiber yarns are staggered and layered inside the profile, tearing along the longitudinal direction of the profile can be effectively avoided under pressure, thus improving the transverse strength of the profile. The transverse reinforcing material includes chopped glass fibers 5 dispersed in the polyurethane resin matrix 1, which can improve the transverse strength of the frame profile. Therefore, the pultruded profile for photovoltaic module frames provided in this embodiment not only has high longitudinal strength, but also high transverse strength, and the overall strength of the profile is excellent.

[0032] In some embodiments of the present invention, the pultruded profile for the photovoltaic module frame comprises, by weight: 20-30 parts of polyurethane resin matrix, 30-60 parts of glass fiber yarn, 5-25 parts of glass fiber, 5-20 parts of glass fiber mat, and 1-10 parts of chopped glass fiber.

[0033] In some embodiments of the present invention, the pultruded profile for the photovoltaic module frame comprises, by weight: 20-25 parts of polyurethane resin matrix, 40-50 parts of glass fiber yarn, 10-20 parts of glass fiber, 10-14 parts of glass fiber mat, and 5-6 parts of chopped glass fiber.

[0034] In some embodiments of the present invention, the pultruded profile for the photovoltaic module frame further comprises, by weight: 0.1-0.1 parts antioxidant, 0.1-1 parts ultraviolet absorber, 0.1-1 parts light stabilizer, 0.1-1 parts water absorber, 0.1-1 parts wetting and dispersing agent, 0.1-1 parts defoamer, and 0.2-2 parts release agent.

[0035] Adjusting the mass ratio of polyurethane resin matrix, glass fiber yarn, glass fiber, glass fiber mat, and chopped glass fiber to an optimal range can improve the strength of the frame profile. Furthermore, adding antioxidants, UV absorbers, and light stabilizers to the polyurethane resin matrix can make the prepared frame profile less prone to yellowing and improve its mechanical properties under prolonged outdoor exposure.

[0036] In some embodiments of the present invention, the polyurethane resin is a polymer of isocyanate and polyol, wherein the isocyanate is selected from at least one of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isoflurane diisocyanate, and dicyclohexylmethane-4,4'-diisocyanate; and the polyol is selected from at least one of polyether polyol and polyester polyol. In some embodiments of the present invention, the antioxidant is selected from phenolic, phosphite, or ketone antioxidants; in some embodiments of the present invention, the ultraviolet absorber is selected from ketone or triazole ultraviolet absorbers. In some embodiments of the present invention, the light stabilizer is selected from ester or phosphite light stabilizers. In some embodiments of the present invention, the water absorbent is a molecular sieve water absorbent. In some embodiments of the present invention, the wetting and dispersing agent and defoamer can be commercially available products from companies such as BYK, Deqian, and Efcona.

[0037] In some embodiments of the present invention, the linear density of the glass fiber yarn is 2400–4800 g / km (specification 2400TEX–4800TEX, i.e., 2400–4800 grams per kilometer of glass fiber yarn); the diameter of the glass fiber is 10–30 μm; alkali-free glass fiber in whole strands can be used, which facilitates traction during manufacturing. The thickness of the glass fiber mat is 0.2–2 mm.

[0038] In some embodiments of the present invention, the diameter of the chopped glass fibers is 10–30 μm, and the length of the chopped glass fibers is 1–5 mm; on any cross-section of the profile: the unit area distribution density F0 of the chopped glass fibers at any position and the unit area distribution density F of the chopped glass fibers at a distance of 10 cm from the position are... 10 The relative deviation (F0-F) 10 The absolute value of ) / F0 does not exceed 20%.

[0039] More preferably, in the pultruded profile for photovoltaic module frames provided by the present invention, the diameter of the chopped glass fibers is 18-25 μm, and the length of the chopped glass fibers is 2-3 mm; on any cross-section of the profile: the relative deviation (F0-F10) between the unit area distribution density F0 of the chopped glass fibers at any position and the unit area distribution density F10 of the chopped glass fibers at a distance of 10 cm from the position. 10 The absolute value of ) / F0 does not exceed 10%.

[0040] In this application, the unit area distribution density of chopped glass fibers refers to the ratio of the area containing chopped glass fibers to the sampled area of ​​a 3cm×3cm square region on the cross-section of the pultruded profile for photovoltaic module frame. By adjusting the center-to-center distance between different sampling regions to 10cm, the unit area distribution density of chopped glass fibers in different regions on the cross-section of the pultruded profile for photovoltaic module frame can be obtained.

[0041] The strength of photovoltaic module frame profiles, especially their lateral strength, is affected by the uniformity of chopped glass fibers distributed within the polyurethane resin matrix. If the distribution of chopped glass fibers is uneven, some areas will have excessively low chopped glass fiber content while others will have excessively high chopped glass fiber content. This uneven distribution not only fails to improve the lateral strength of the polyurethane resin matrix but may even have a negative effect, reducing it. Provided the chopped glass fiber content is within a certain range, the diameter and length of the selected chopped glass fibers directly affect their uniformity of distribution within the polyurethane resin matrix. When the diameter and length of the chopped glass fibers are within the preferred range provided by this invention, their uniformity of distribution within the polyurethane resin matrix can be significantly improved, thereby significantly increasing the strength of the frame profile.

[0042] Some embodiments of the present invention provide a photovoltaic module frame, which is prepared using a pultruded profile for photovoltaic module frames provided in the first aspect of the present invention.

[0043] Figure 2 A process flow diagram of the manufacturing process of a photovoltaic module frame according to an embodiment of the present invention is shown, including the following steps: S1: The polyol, the raw material for the preparation of the polyurethane resin, and the additives in the profile are stirred and mixed in a mixing tank, the chopped glass fibers are added, and stirring is continued to obtain a resin premix in which the chopped glass fibers are uniformly dispersed; S2: The glass fiber yarn, the glass fiber, and the glass fiber mat are fed through a yarn feeding device, shaped through a yarn threading mold to obtain the longitudinal reinforcement material, and guided into a resin tank through a guiding device; S3: The resin premix and the isocyanate, the raw material for the preparation of the polyurethane resin, are mixed in proportion and injected into the resin tank through a glue injection machine to impregnate the longitudinal reinforcement material, and pre-cured by heating; S4: The pre-cured product is cured in a heating molding mold; S5: The formed photovoltaic module frame pultruded profile is pulled out from the outlet of the heating molding mold by a traction device and cut into photovoltaic module frames suitable for the size of photovoltaic laminates.

[0044] Since the pultruded profile for photovoltaic module frames according to the present invention has good longitudinal and transverse strength, the photovoltaic module frames made from this profile also have good longitudinal and transverse strength and will not tear along the longitudinal direction of the profile under pressure.

[0045] Figure 3 This is a three-dimensional structural diagram of a photovoltaic module frame according to an embodiment of the present invention. Figure 3As shown, the photovoltaic module frame includes a receiving groove 20 for mounting photovoltaic module laminates and a support portion 21 located below the receiving groove 20. The bottom of the receiving groove 20 and the top of the support portion 21 share a top bearing surface 22. The receiving groove 20 also includes a first limiting surface 23 and a second limiting surface 24. The first limiting surface 23, the second limiting surface 24 and the top bearing surface 22 are sequentially joined together to form the receiving groove 20. The receiving groove 20 is open on one side. The support portion 21 also includes a first side surface 25, a second side surface 26 and a bottom bearing surface 27. The top bearing surface 22, the first side surface 25, the bottom bearing surface 27 and the second side surface 26 are sequentially joined together to form a closed cavity 28.

[0046] Figure 4 This is a three-dimensional structural diagram of a photovoltaic module frame according to another embodiment of the present invention. Figure 4 As shown, the photovoltaic module frame includes a receiving groove 30 for mounting photovoltaic module laminates and a support portion 31 located below the receiving groove 30. The bottom of the receiving groove 30 and the top of the support portion 31 share a top bearing surface 32. The receiving groove 30 also includes a first limiting surface 33 and a second limiting surface 34. The first limiting surface 33, the second limiting surface 34 and the top bearing surface 32 are sequentially joined together to form the receiving groove 30. The receiving groove 30 is open on one side. The support portion 31 also includes a first side surface 35 and a bottom bearing surface 36. The top bearing surface 32, the first side surface 35 and the bottom bearing surface 36 are sequentially joined together to form an open cavity 37. The opening direction of the open cavity 37 is opposite to the opening direction of the receiving groove 30.

[0047] The advantages of this application are further illustrated below with specific embodiments and comparative examples. Unless otherwise specified, all materials used are commercially available products. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of this application.

[0048] Examples 1-10

[0049] S1: The polyether polyol and additives are stirred and mixed in a mixing tank, then chopped glass fibers are added, and stirring is continued to obtain a resin premix in which the chopped glass fibers are uniformly dispersed. The additives, by weight, comprise: 0.1 parts antioxidant, 1 part UV absorber, 1 part light stabilizer, 1 part water absorber, 1 part wetting and dispersing agent, 1 part defoamer, and 2 parts release agent. The weight percentages of the polyether polyol, the weight percentages of the chopped glass fibers, their diameter and length, and the relative deviations of the chopped glass fiber density per unit area F10 on the cross-section of the profile are shown in Table 1.

[0050] S2: Glass fiber yarn, glass fiber, and glass fiber mat are fed into the resin tank via a yarn feeding device, shaped through a yarn threading die to obtain longitudinal reinforcing material, and then guided into the resin tank via a guiding device. The glass fiber yarn is 4800 TEX; it uses whole strands of alkali-free glass fiber with a diameter of 20 μm per fiber; the glass fiber mat is 1 mm thick. The mass fractions of the glass fiber yarn, glass fiber, and glass fiber mat are shown in Table 1.

[0051] S3: Mix the resin premix and isocyanate in a certain proportion, inject the mixture into the resin tank through a dispensing machine to impregnate the longitudinal reinforcing material, and heat to pre-cure;

[0052] S4: The pre-cured product is cured in a thermoforming mold. After curing, the longitudinal reinforcement material is distributed in the profile as follows: the longitudinal reinforcement material includes glass fiber yarns, glass fibers, and glass fiber mats that extend continuously in the longitudinal direction of the profile; on any cross-section of the profile: the glass fiber yarns are interlaced, the glass fibers are densely distributed between the glass fiber yarns, and the glass fiber mats wrap around the outer periphery of the profile cross-section. The above distribution pattern is achieved by adjusting the yarn threading mold structure.

[0053] S5: Pull out the pultruded profile for the photovoltaic module frame from the outlet of the heating and forming mold using a traction device, and cut it into a photovoltaic module frame suitable for the size of the photovoltaic laminate.

[0054] Comparative Examples 1-3

[0055] The profile prepared in Comparative Example 1 has no glass fiber yarn in the longitudinal reinforcement material.

[0056] The profile prepared in Comparative Example 2 also contains glass fiber yarn as the longitudinal reinforcement material, but the glass fiber yarn is not interlaced.

[0057] The profile prepared in Comparative Example 3 does not contain chopped glass fibers as transverse reinforcement.

[0058] Bending performance test:

[0059] The pultruded profiles for photovoltaic module frames prepared in Examples 1-10 and Comparative Examples 1-3 were tested for longitudinal and transverse strength in accordance with GB / T1449-2005 Test Method for Bending Properties of Glass Fiber Reinforced Plastics.

[0060] The preparation parameters and bending performance test results of the pultruded profiles for photovoltaic module frames prepared in Examples 1-10 and Comparative Examples 1-3 are shown in Table 1.

[0061] Table 1. Preparation parameters and bending performance test results

[0062]

[0063] As shown in Table 1, the pultruded profiles for photovoltaic module frames prepared in Examples 1-10 all include a polyurethane resin matrix and reinforcing materials impregnated in the polyurethane resin matrix. These reinforcing materials include glass fiber yarns, glass fibers, and glass fiber mats continuously extending in the longitudinal direction of the profile, as well as chopped glass fibers dispersed in the profile. The pultruded profiles for photovoltaic module frames prepared in Examples 1-10, after bending performance tests, showed significantly better overall strength performance than the profiles in Comparative Examples 1-3. The profile prepared in Comparative Example 1 did not contain glass fiber yarn reinforcement, resulting in lower longitudinal and transverse strength. Although the profile prepared in Comparative Example 2 contained glass fiber yarn reinforcement, the glass yarn was not interlaced, thus improving longitudinal strength but not significantly improving transverse strength, resulting in a large gap compared to the profiles in Examples 1-10. The profile in Comparative Example 3 did not contain chopped glass fiber reinforcement, therefore its transverse strength was also lower than that of the profiles in Examples 1-10.

[0064] Examples 1-4 also illustrate the effect of variations in the mass ratio of the polyurethane resin matrix and its internal reinforcing materials on the strength of the profiles. In Example 1, the proportion of chopped glass fibers in the polyurethane was too small, resulting in greater randomness in their dispersion within the polyurethane and an inability to achieve uniform distribution. In Example 3, the proportion of chopped glass fibers in the polyurethane was too large, leading to easy aggregation during preparation and achieving optimal distribution uniformity, thus affecting the strength improvement. Compared to Examples 1-2, the profiles prepared in Examples 3-4 exhibited superior longitudinal and transverse strength because the mass ratio of the polyurethane resin matrix and reinforcing materials was within the preferred range provided by this invention.

[0065] Examples 5-10 illustrate the influence of the diameter, length, and distribution uniformity of chopped glass fibers on the profile strength. In Example 5, the diameter and length of the chopped glass fibers were too small, resulting in significant random dispersion and thus reduced uniformity. In Example 10, the diameter and length of the chopped glass fibers were too large, increasing the difficulty of achieving uniform distribution and also reducing uniformity. The transverse strength of the profiles in Examples 5 and 10 was not optimal. However, Examples 6-9, due to the suitable diameter and length of the chopped glass fibers, showed a significant improvement in transverse strength.

[0066] The above examples are merely illustrative of the technical concept and features of this invention, intended to enable those skilled in the art to understand the content of this invention and implement it accordingly, and should not be construed as limiting the scope of protection of this invention. All equivalent transformations or modifications made according to the spirit and essence of this invention should be included within the scope of protection of this invention.

Claims

1. A pultruded profile for a photovoltaic module frame, characterized in that, The profile includes a polyurethane resin matrix and longitudinal and transverse reinforcing materials impregnated in the polyurethane resin matrix; The longitudinal reinforcing material includes glass fiber yarns, glass fibers, and glass fiber mats that extend continuously in the longitudinal direction of the profile; on any cross-section of the profile: the glass fiber yarns are interlaced and stacked, the glass fibers are densely distributed between the glass fiber yarns, and the glass fiber mats are wrapped around the outer periphery of the cross-section of the profile. The transverse reinforcing material comprises short-cut glass fibers dispersed in the polyurethane resin matrix; The diameter of the chopped glass fiber is 10~30μm, and the length of the chopped glass fiber is 1~5mm; On any cross-section of the profile: the unit area distribution density F0 of chopped glass fibers at any position and the unit area distribution density F of chopped glass fibers at a distance of 10 cm from the stated position. 10 The relative deviation (F0-F) 10 The absolute value of F0 does not exceed 20%.

2. The pultruded profile for photovoltaic module frames according to claim 1, characterized in that, It contains, by weight, 20-30 parts of polyurethane resin matrix, 30-60 parts of glass fiber yarn, 5-25 parts of glass fiber, 5-20 parts of glass fiber mat, and 1-10 parts of chopped glass fiber.

3. The pultruded profile for photovoltaic module frames according to claim 2, characterized in that, It contains, by weight, 20-25 parts of polyurethane resin matrix, 40-50 parts of glass fiber yarn, 10-20 parts of glass fiber, 10-14 parts of glass fiber mat, and 5-6 parts of chopped glass fiber.

4. The pultruded profile for photovoltaic module frames according to claim 2, characterized in that, It also contains, by weight, 0.1 parts antioxidant, 0.1 to 1 part ultraviolet absorber, 0.1 to 1 part light stabilizer, 0.1 to 1 part water absorber, 0.1 to 1 part wetting and dispersing agent, 0.1 to 1 part defoamer, and 0.2 to 2 parts release agent.

5. The pultruded profile for photovoltaic module frames according to claim 1, characterized in that, The linear density of the glass fiber yarn is 2400~4800 g / km; The diameter of the glass fiber is 10~30μm; The thickness of the glass fiber mat is 0.2~2mm.

6. The pultruded profile for photovoltaic module frames according to claim 1, characterized in that, The chopped glass fibers have a diameter of 18~25μm and a length of 2~3mm; On any cross-section of the profile: the unit area distribution density F0 of chopped glass fibers at any position and the unit area distribution density F of chopped glass fibers at a distance of 10 cm from the stated position. 10 The relative deviation (F0-F) 10 The absolute value of F0 does not exceed 10%.

7. The pultruded profile for photovoltaic module frames according to claim 4, characterized in that, The polyurethane resin is a polymer of isocyanate and polyol, wherein the isocyanate is selected from at least one of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isoflurone diisocyanate and dicyclohexylmethane-4,4'-diisocyanate; and the polyol is selected from at least one of polyether polyol and polyester polyol. The antioxidant is selected from phenolic, phosphite, or ketone antioxidants; The ultraviolet absorber is selected from ketone or triazole ultraviolet absorbers; The light stabilizer is selected from ester or phosphite light stabilizers; The absorbent is a molecular sieve absorbent.

8. A photovoltaic module frame, characterized in that, The pultruded profile is prepared using any one of claims 1 to 7.

9. The photovoltaic module frame according to claim 8, characterized in that, It includes a receiving groove for installing photovoltaic module laminates and a support portion located below the receiving groove, wherein the bottom of the receiving groove and the top of the support portion share a top bearing surface; The receiving groove further includes a first limiting surface and a second limiting surface, which are sequentially joined together to form the receiving groove, and the receiving groove is open on one side. The support portion also includes a first side surface, a bottom bearing surface, and a second side surface, which are sequentially joined together to form a closed cavity.

10. The photovoltaic module frame according to claim 8, characterized in that, It includes a receiving groove for installing photovoltaic module laminates and a support portion located below the receiving groove, wherein the bottom of the receiving groove and the top of the support portion share a top bearing surface; The receiving groove further includes a first limiting surface and a second limiting surface, which are sequentially joined together to form the receiving groove, and the receiving groove is open on one side. The support portion also includes a first side surface and a bottom bearing surface. The top bearing surface, the first side surface, and the bottom bearing surface are sequentially joined together to form an open cavity. The opening direction of the cavity is opposite to the opening direction of the receiving groove.

11. The method for preparing a photovoltaic module frame according to claim 9 or 10, characterized in that, Includes the following steps: S1: The polyol, the raw material for preparing the polyurethane resin, and the additives in the profile are stirred and mixed in a mixing tank. The chopped glass fibers are added and stirring is continued to obtain a resin premix in which the chopped glass fibers are uniformly dispersed. S2: The glass fiber yarn, the glass fiber, and the glass fiber mat are fed through a yarn feeding device, shaped through a yarn threading mold to obtain the longitudinal reinforcing material, and then guided into a resin tank through a guiding device; S3: Mix the resin premix and the isocyanate, the raw material for preparing the polyurethane resin, in a certain proportion, and inject the mixture into the resin tank through a dispensing machine to impregnate the longitudinal reinforcing material, and then heat and pre-cur it. S4: The pre-cured product is cured in a thermoforming mold; S5: Pull out the pultruded profile for the photovoltaic module frame from the outlet of the heating and forming mold using a traction device, and cut it into a photovoltaic module frame suitable for the size of the photovoltaic laminate.

Citation Information

Patent Citations

  • Fiber-felt-reinforced composite material solar energy assembly frame and preparation method thereof

    CN104760299A

  • Short-fiber-reinforced pultrusion composite material solar energy assembly frame and preparation method thereof

    CN104761880A