A method for preparing pyridine-modified graphite phase carbon nitride film electrode

The graphite phase carbon nitride thin film electrode is modified by pyridine solvothermally, which solves the serious problem of photogenerated carrier recombination in the graphite phase carbon nitride thin film electrode, increases the photocurrent density and electrochemical active area, and improves the photoelectrochemical performance.

CN115627498BActive Publication Date: 2024-10-18CHINA THREE GORGES UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211242792.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-11
Publication Date
2024-10-18
Estimated Expiration
2042-10-11

AI Technical Summary

Technical Problem

Existing graphite-phase carbon nitride film electrodes suffer from serious recombination of photogenerated carriers during photoelectrocatalytic decomposition of water, resulting in photoelectrochemical performance lower than the theoretical current value, and traditional methods are not environmentally friendly and energy-saving.

Method used

A pyridine solvothermal modified graphite phase carbon nitride film electrode preparation method is used. A pyridine solution is added to the graphite phase carbon nitride film for solvothermal treatment to regulate its crystallinity and electrochemical active area and inhibit the recombination of photogenerated carriers.

Benefits of technology

Significantly improve the photocurrent density of graphite phase carbon nitride, increase the electrochemical active area, weaken the fluorescence effect and photogenerated electron hole pair recombination, and improve the photoelectrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 221008093430
    Figure 221008093430
  • Figure 221008093433
    Figure 221008093433
  • Figure 221008093436
    Figure 221008093436
Patent Text Reader

Abstract

The present invention belongs to the field of photoelectrochemistry and thin film manufacturing, and relates to a method for preparing a pyridine solvent-thermal modified graphite phase carbon nitride film. The preparation of the pyridine solvent-thermal modified graphite phase carbon nitride film electrode includes weighing a certain amount of dicyandiamide and cyanuric acid, preparing a graphite phase carbon nitride film on a conductive glass by chemical vapor deposition; then immersing the graphite phase carbon nitride film in a pyridine solution, and using a solvent-thermal reaction to obtain a pyridine-modified graphite phase carbon nitride film electrode. The pyridine-modified graphite phase carbon nitride film electrode prepared by the present invention realizes crystallinity regulation and increases the electrochemical active area; on the other hand, after pyridine solvent-thermal modification, the photocurrent density is significantly improved compared to the original graphite phase carbon nitride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photoelectrochemistry and relates to a method for preparing a pyridine-modified graphite phase carbon nitride film electrode. Background Art

[0002] Environmental pollution, energy shortage and other issues seriously threaten human survival and safety, so new energy must be developed to get out of the predicament. Among many new energy sources, hydrogen energy has gained people's favor due to its own advantages such as no pollution and high calorific value. Traditional industrial production of hydrogen is generally prepared by water gas method and electrolysis, but these two methods are not energy-saving and environmentally friendly. Therefore, it is urgent to develop clean production technology of hydrogen.

[0003] Photoelectrocatalytic water splitting technology produces hydrogen by absorbing light through photoanode materials. This technology is clean and pollution-free, and is in line with the concept of sustainable development. As a photoelectrocatalyst, graphite carbon nitride has the advantages of suitable band gap, good stability and low price. At present, researchers have been able to prepare graphite carbon nitride thin film electrodes through thermal vapor deposition, microcontact printing, hydrothermal and other methods, but due to the serious recombination of photogenerated carriers (Angew.Chem. Int. Ed. 2019, 58, 6138–6151). In recent years, researchers have used prefabricated seed layers, scraper blades, copolymerization and molecular grafting to regulate the crystallinity, defects and electrochemical active area of ​​materials to inhibit photogenerated carrier recombination, which has improved its photoelectrochemical performance to a certain extent, but its photoelectrochemical performance is still far lower than its theoretical current value. (Angew.Chem. 2018, 130, 1200–1206; Journal of Materials Chemistry A, 2020, 8(41):21474-21502; Journal of Colloid and Interface Science. 2020, 578:574-583.) This method first prepares a graphite carbon nitride film and then thermally modifies the graphite carbon nitride by pyridine solvent. Unlike molecular grafting, this method does not connect the pyridine molecules with the graphite carbon nitride, but instead achieves the regulation of the crystallinity and electrochemical active area of ​​the graphite carbon nitride, ultimately effectively inhibiting the recombination of photogenerated carriers and promoting the improvement of the photoelectrochemical performance. Summary of the invention

[0004] According to the shortcomings of the existing photoelectric catalytic material graphite phase carbon nitride, the present invention provides a method for preparing a pyridine-modified graphite phase carbon nitride film electrode.

[0005] The present invention is achieved through the following technical scheme: a method for preparing a pyridine-modified graphite phase carbon nitride film electrode, the specific process is as follows.

[0006] First, add appropriate amounts of dicyandiamide and cyanuric acid into a mortar, and after grinding, evenly spread the powder in a porcelain boat, then put a piece of conductive glass on the powder, and then cover the porcelain boat with aluminum foil, and finally put it into a tube furnace, react at a certain temperature under the protection of inert gas, keep warm for a certain period of time, cool down, wash and dry, and then obtain a graphite phase carbon nitride film electrode;

[0007] In the second step, the graphite phase carbon nitride film electrode is placed in a reactor containing a certain volume of pyridine solution, heated to a certain temperature, kept at a constant temperature for 4 to 8 hours, and cooled to room temperature to obtain pyridine-modified graphite phase carbon nitride.

[0008] The mass ratio of dicyandiamide to cyanuric acid is 1:0.1-10.

[0009] The conductive glass includes but is not limited to FTO and ITO.

[0010] The inert gas includes nitrogen and argon.

[0011] The reaction temperature in the furnace at a certain temperature is 450-550°C.

[0012] The pyridine solution is a pure solution of pyridine compounds.

[0013] The volume of the certain amount of pyridine accounts for about 40-80% of the volume of the reactor.

[0014] The pyridine solvent thermal reaction temperature ranges from 110 to 180°C.

[0015] The pyridine solvent thermal reaction preferably takes 4 to 8 hours.

[0016] The graphite phase carbon nitride is a graphite phase carbon nitride film electrode with a low degree of crystallization and a large electrochemical active area.

[0017] The beneficial effects of the present invention are:

[0018] The pyridine-modified graphite phase carbon nitride film of the present invention has the following advantages:

[0019] (1) The crystallinity of graphite carbon nitride treated by this experimental method is reduced and the electrochemical active area is increased.

[0020] (2) The photocurrent density of the optimal pyridine-modified graphite carbon nitride prepared by the present invention is increased by 132% compared with the current density of the initial graphite carbon nitride, indicating that pyridine modification can improve the photoelectric properties of graphite carbon nitride.

[0021] (3) Compared with the original graphite phase carbon nitride, the fluorescence effect of the pyridine-modified graphite phase carbon nitride is weakened, the recombination of photogenerated electron-hole pairs is weakened, and the photoelectric performance is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Shown are the SEM images of the samples prepared in Examples 1 and 9.

[0023] Figure 2 Shown are the XRD patterns of the samples prepared in Examples 1 and 9.

[0024] Figure 3 Shown are the photoresponse current spectra of the samples prepared in Examples 1 to 9.

[0025] Figure 4 Shown are the PL spectra of the samples prepared in Examples 1 and 2.

[0026] Figure 5 Shown are the EIS spectra of the samples prepared in Examples 1 and 2.

[0027] Figure 6 Shown are the ECSA spectra of the samples prepared in Examples 1 and 9. DETAILED DESCRIPTION

[0028] The specific implementation method of preparing pyridine-modified graphite phase carbon nitride is as follows:

[0029] Example 1

[0030] Weigh 2.67g of dicyandiamide and 1.33g of cyanuric acid, pour the weighed drugs into a mortar for grinding, and move the drugs into a porcelain boat after grinding for 3 minutes. At this time, spread the drugs evenly in the porcelain boat. Subsequently, the ultrasonically cleaned FTO glass is dried and gently placed in the middle of the porcelain boat, with the conductive surface of the FTO glass facing up; then the porcelain boat is completely coated with aluminum foil, and then placed in a tubular furnace for high-temperature reaction, wherein the temperature of the tubular furnace is 550°C, the heating rate is 5°C / min, the insulation time is 2h, and the insulation temperature is 550°C. After the furnace is cooled, graphite phase carbon nitride can be obtained, which is recorded as CN.

[0031] Example 2

[0032] Weigh 2.67g dicyandiamide and 1.33g cyanuric acid, pour the weighed drugs into the mortar for grinding, and move the drugs into the porcelain boat after grinding for 3 minutes, and then evenly spread the drugs in the porcelain boat. Then, dry the ultrasonically cleaned FTO glass and gently place it in the middle of the porcelain boat, with the conductive surface of the FTO glass facing up; then wrap the porcelain boat completely with aluminum foil, and then put it into a tube furnace for high-temperature reaction, where the temperature of the tube furnace is 550℃, the heating rate is 5℃ / min, the insulation time is 2h, and the insulation temperature is 550℃. After the furnace is cooled, graphite phase carbon nitride can be obtained, and then the graphite phase carbon nitride can be placed in the reactor, where the FTO conductive surface (containing graphite phase carbon nitride film) is placed obliquely downward; then add 13ml of pyridine solvent to the reactor in the fume hood, the solvent thermal reaction temperature is 160℃, and the solvent thermal reaction time is 6h. After cooling, the FTO glass was rinsed twice with deionized water, cleaned once with anhydrous ethanol, and dried to obtain pyridine-modified graphite phase carbon nitride thin film electrodes, which were recorded as CN-P, CN-P-160, CN-P-13, and CN-P-6.

[0033] Example 3

[0034] Weigh 2.67g dicyandiamide and 1.33g cyanuric acid, pour the weighed drugs into the mortar for grinding, and move the drugs into the porcelain boat after grinding for 3 minutes, and then evenly spread the drugs in the porcelain boat. Then, dry the ultrasonically cleaned FTO glass and gently place it in the middle of the porcelain boat, with the conductive surface of the FTO glass facing up; then wrap the porcelain boat completely with aluminum foil, and then put it into a tube furnace for high-temperature reaction, where the temperature of the tube furnace is 550℃, the heating rate is 5℃ / min, the insulation time is 2h, and the insulation temperature is 550℃. After the furnace is cooled, graphite phase carbon nitride can be obtained, and then the graphite phase carbon nitride can be placed in the reactor, where the FTO conductive surface (containing graphite phase carbon nitride film) is placed obliquely downward; then add 13ml of pyridine solvent to the reactor in the fume hood, the solvent thermal reaction temperature is 140℃, and the solvent thermal reaction time is 6h. After cooling, the FTO glass was rinsed twice with deionized water, cleaned once with anhydrous ethanol, and dried to obtain a pyridine-modified graphite phase carbon nitride thin film electrode, which was recorded as CN-P-140.

[0035] Example 4

[0036] Weigh 2.67 g of dicyandiamide and 1.33 g of cyanuric acid, pour the weighed drugs into the mortar for grinding, and move the drugs into the porcelain boat after grinding for 3 minutes, and then evenly spread the drugs in the porcelain boat. Then, dry the ultrasonically cleaned FTO glass and gently place it in the middle of the porcelain boat, with the conductive surface of the FTO glass facing up; then wrap the porcelain boat completely with aluminum foil, and then put it into a tube furnace for high-temperature reaction, where the temperature of the tube furnace is 550 ° C, the heating rate is 5 ° C / min, the insulation time is 2h, and the insulation temperature is 550 ° C. After the furnace is cooled, graphite phase carbon nitride can be obtained, and then the graphite phase carbon nitride can be placed in the reactor, where the FTO conductive surface (containing graphite phase carbon nitride film) is placed obliquely downward; then add 13 ml of pyridine solvent to the reactor in the fume hood, the solvent thermal reaction temperature is 150 ° C, and the solvent thermal reaction time is 6h. After cooling, the FTO glass was rinsed twice with deionized water, cleaned once with anhydrous ethanol, and dried to obtain a pyridine-modified graphite phase carbon nitride thin film electrode, which was recorded as CN-P-150.

[0037] Example 5

[0038] Weigh 2.67 g of dicyandiamide and 1.33 g of cyanuric acid, pour the weighed drugs into the mortar for grinding, and move the drugs into the porcelain boat after grinding for 3 minutes, and then evenly spread the drugs in the porcelain boat. Then, dry the ultrasonically cleaned FTO glass and gently place it in the middle of the porcelain boat, with the conductive surface of the FTO glass facing up; then wrap the porcelain boat completely with aluminum foil, and then put it into a tube furnace for high-temperature reaction, where the temperature of the tube furnace is 550 ° C, the heating rate is 5 ° C / min, the insulation time is 2h, and the insulation temperature is 550 ° C. After the furnace is cooled, graphite phase carbon nitride can be obtained, and then the graphite phase carbon nitride can be placed in the reactor, where the FTO conductive surface (containing graphite phase carbon nitride film) is placed obliquely downward; then add 13 ml of pyridine solvent to the reactor in the fume hood, the solvent thermal reaction temperature is 170 ° C, and the solvent thermal reaction time is 6h. After cooling, the FTO glass was rinsed twice with deionized water, cleaned once with anhydrous ethanol, and dried to obtain a pyridine-modified graphite phase carbon nitride thin film electrode, which was recorded as CN-P-170.

[0039] Example 6

[0040] Weigh 2.67 g of dicyandiamide and 1.33 g of cyanuric acid, pour the weighed drugs into the mortar for grinding, and move the drugs into the porcelain boat after grinding for 3 minutes, and then evenly spread the drugs in the porcelain boat. Then, dry the ultrasonically cleaned FTO glass and gently place it in the middle of the porcelain boat, with the conductive surface of the FTO glass facing up; then wrap the porcelain boat completely with aluminum foil, and then put it into a tube furnace for high-temperature reaction, where the temperature of the tube furnace is 550 ° C, the heating rate is 5 ° C / min, the insulation time is 2h, and the insulation temperature is 550 ° C. After the furnace is cooled, graphite phase carbon nitride can be obtained, and then the graphite phase carbon nitride can be placed in the reactor, where the FTO conductive surface (containing graphite phase carbon nitride film) is placed obliquely downward; then add 13 ml of pyridine solvent to the reactor in the fume hood, the solvent thermal reaction temperature is 160 ° C, and the solvent thermal reaction time is 4h. After cooling, the FTO glass was rinsed twice with deionized water, cleaned once with anhydrous ethanol, and dried to obtain a pyridine-modified graphite phase carbon nitride thin film electrode, CN-P-4.

[0041] Example 7

[0042] Weigh 2.67g dicyandiamide and 1.33g cyanuric acid, pour the weighed drugs into the mortar for grinding, and move the drugs into the porcelain boat after grinding for 3 minutes, and then evenly spread the drugs in the porcelain boat. Then, dry the ultrasonically cleaned FTO glass and gently place it in the middle of the porcelain boat, with the conductive surface of the FTO glass facing up; then wrap the porcelain boat completely with aluminum foil, and then put it into a tube furnace for high-temperature reaction, where the temperature of the tube furnace is 550℃, the heating rate is 5℃ / min, the insulation time is 2h, and the insulation temperature is 550℃. After the furnace is cooled, graphite phase carbon nitride can be obtained, and then the graphite phase carbon nitride can be placed in the reactor, where the FTO conductive surface (containing graphite phase carbon nitride film) is placed obliquely downward; then add 13ml of pyridine solvent to the reactor in the fume hood, the solvent thermal reaction temperature is 160℃, and the solvent thermal reaction time is 8h. After cooling, the FTO glass was rinsed twice with deionized water, cleaned once with anhydrous ethanol, and dried to obtain a pyridine-modified graphite phase carbon nitride thin film electrode, which was recorded as CN-P-8.

[0043] Example 8

[0044] Weigh 2.67g dicyandiamide and 1.33g cyanuric acid, pour the weighed drugs into the mortar for grinding, and move the drugs into the porcelain boat after grinding for 3 minutes, and then evenly spread the drugs in the porcelain boat. Then, dry the ultrasonically cleaned FTO glass and gently place it in the middle of the porcelain boat, with the conductive surface of the FTO glass facing up; then wrap the porcelain boat completely with aluminum foil, and then put it into a tube furnace for high-temperature reaction, where the temperature of the tube furnace is 550℃, the heating rate is 5℃ / min, the insulation time is 2h, and the insulation temperature is 550℃. After the furnace is cooled, graphite phase carbon nitride can be obtained, and then the graphite phase carbon nitride can be placed in the reactor, where the FTO conductive surface (containing graphite phase carbon nitride film) is placed obliquely downward; then add 12ml of pyridine solvent to the reactor in the fume hood, the solvent thermal reaction temperature is 160℃, and the solvent thermal reaction time is 6h. After cooling, the FTO glass was rinsed twice with deionized water, cleaned once with anhydrous ethanol, and dried to obtain a pyridine-modified graphite phase carbon nitride thin film electrode, which was recorded as CN-P-12.

[0045] Example 9

[0046] Weigh 2.67g dicyandiamide and 1.33g cyanuric acid, pour the weighed drugs into the mortar for grinding, and move the drugs into the porcelain boat after grinding for 3 minutes, and then evenly spread the drugs in the porcelain boat. Then, dry the ultrasonically cleaned FTO glass and gently place it in the middle of the porcelain boat, with the conductive surface of the FTO glass facing up; then wrap the porcelain boat completely with aluminum foil, and then put it into a tube furnace for high-temperature reaction, where the temperature of the tube furnace is 550℃, the heating rate is 5℃ / min, the insulation time is 2h, and the insulation temperature is 550℃. After the furnace is cooled, graphite phase carbon nitride can be obtained, and then the graphite phase carbon nitride can be placed in the reactor, where the FTO conductive surface (containing graphite phase carbon nitride film) is placed obliquely downward; then add 14ml of pyridine solvent to the reactor in the fume hood, the solvent thermal reaction temperature is 160℃, and the solvent thermal reaction time is 6h. After cooling, the FTO glass was rinsed twice with deionized water, cleaned once with anhydrous ethanol, and dried to obtain a pyridine-modified graphite phase carbon nitride thin film electrode, which was recorded as CN-P-14.

[0047] Morphological Characterization of Graphitic Carbon Nitride Solvothermally Modified by Pyridine

[0048] By performing scanning electron microscopy (SEM) analysis on the photoelectrocatalysts prepared in Example 1 and Example 9, the morphological structures of the two samples were obtained, as shown in FIG. Figure 1As shown, (a) and (c), (b) and (d) are the morphological images of graphite phase carbon nitride and pyridine solvent-thermal modified graphite phase carbon nitride observed at 2000 and 20000 times magnification respectively. The surface morphology of pyridine-modified graphite phase carbon nitride has changed compared with the original graphite phase carbon nitride. Its surface is rougher and irregular, with more rod-like stacking structures, and the rod size is larger than that of the original graphite phase carbon nitride. The surface of graphite phase carbon nitride has block stacking and some rod-like structures, which is relatively flat.

[0049] Structural Characterization of Graphitic Carbon Nitride Solvothermally Modified by Pyridine

[0050] Figure 2 It is the X-ray diffraction pattern of the photoelectric catalyst prepared in Example 1 and Example 2. Compared with the initial graphite phase carbon nitride, the two diffraction peaks of the pyridine solvent-thermal modified graphite phase carbon nitride are 12.9° and 27.4°, and these two diffraction peaks correspond to the (100) and (002) crystal planes of the graphite phase carbon nitride, respectively. The position of the diffraction peak did not change before and after the pyridine treatment, indicating that the pyridine solvent thermal treatment did not change the structure of the graphite phase carbon nitride. At the same time, the diffraction peak width of the graphite phase carbon nitride after pyridine solvent thermal treatment increased and the intensity weakened, indicating that the crystallinity is poor and there are more defects.

[0051] Performance Analysis of Graphite Carbon Nitride Modified by Pyridine Solvothermally

[0052] Figure 3 The photocurrent diagrams of the photoelectrocatalysts prepared in Examples 1~9 measured by linear voltammetry scanning method. Figure 3 (a), (b), and (c) are the optimal experiments for the three conditions of temperature, volume, and time. It can be seen from the figure that the photocurrent density of the pyridine solvent thermally modified graphite phase carbon nitride obtained in the experiment is the largest when the temperature is 160°C, the volume is 13ml, and the time is 6h, reaching 35.3μA*cm -2 . Figure 3 (d) The current density of the original graphite phase carbon nitride in the figure is 15.2μA*cm -2 The photocurrent density of the graphite phase carbon nitride modified by pyridine increased by 132% compared with that of the original graphite phase carbon nitride. The increase in the photocurrent density of the graphite phase carbon nitride modified by pyridine indicates that the recombination of electron-hole pairs is weakened, which is conducive to the improvement of photoelectrocatalytic performance.

[0053] Figure 4 The fluorescence spectra of Example 1 and Example 2 are shown. The fluorescence intensity of the graphite phase carbon nitride modified with pyridine is weaker than that of the original graphite phase carbon nitride, indicating that the electron-hole recombination of the modified graphite phase carbon nitride is weakened and the separation efficiency is improved.

[0054] Figure 5The electrochemical impedance spectra of Example 1 and Example 2. The arc radius of the graphite phase carbon nitride modified by pyridine is smaller, indicating that its carrier migration rate is faster, which can effectively inhibit the recombination of photogenerated electron-hole pairs, thereby improving the photoelectrocatalytic performance of the material.

[0055] Figure 6 The electrochemically active area (ECSA) spectra of Example 1 and Example 2 are shown in Figure 1. The electrochemically active area is determined by calculating the double-layer capacitance of the material. The double-layer capacitance of the original graphite phase carbon nitride is 3.28 μF, and the double-layer capacitance of the graphite phase carbon nitride after pyridine solvent thermal modification is 6.46 μF. The electrochemically active area is 97% higher than that of the original graphite phase carbon nitride. A higher active electrochemical area indicates that the material has better catalytic performance.

[0056] The above-mentioned invention examples do not cover all the contents of this invention, so the present invention cannot be limited to them. Although the embodiments of the present invention have been described in detail, ordinary technicians in the same field can still modify and replace the present invention; and all technical solutions and improvements that do not deviate from the spirit and scope of the present invention should be covered within the legal protection scope of the present invention.

Claims

1. A method for preparing a pyridine-modified graphite phase carbon nitride thin film electrode, characterized in that: The following steps are involved: The first step is to add an appropriate amount of dicyandiamide and cyanuric acid into a mortar, and after grinding, evenly spread the powder in a porcelain boat, then put a piece of conductive glass on the powder, and then cover the porcelain boat with aluminum foil, and finally put it into a tube furnace, react at a certain temperature under the protection of inert gas, keep warm for a certain period of time, cool down, wash and dry, and obtain a graphite phase carbon nitride film electrode; In the second step, the graphite phase carbon nitride film electrode is placed in a reactor containing a certain volume of pyridine solution, the temperature is raised to a certain temperature, the temperature is kept constant for 4 to 8 hours, and the temperature is cooled to room temperature to obtain pyridine-modified graphite phase carbon nitride; the pyridine solution is a pure solution of pyridine compounds; the volume of the certain amount of pyridine accounts for 40 to 80% of the volume of the reactor; the temperature range of the pyridine solvent thermal reaction is 110 to 180°C.

2. The method for preparing a pyridine-modified graphite phase carbon nitride thin film electrode according to claim 1, characterized in that: The mass ratio of dicyandiamide to cyanuric acid is 1:0.1-10.

3. The method for preparing a pyridine-modified graphite phase carbon nitride thin film electrode according to claim 1, characterized in that: The conductive glass includes but is not limited to FTO and ITO.

4. The method for preparing a pyridine-modified graphite phase carbon nitride thin film electrode according to claim 1, characterized in that: The inert gas includes nitrogen and argon.

5. The method for preparing a pyridine-modified graphite phase carbon nitride thin film electrode according to claim 1, characterized in that: The reaction temperature in the furnace at a certain temperature is 450-550°C.

Citation Information

Patent Citations

  • Preparation method of WO3 nanosheet photoelectrode modified by dipyridyl-cobalt

    CN106757123A

  • Quantum dot sensitized solar cell with graphite phase carbon nitride interface layer and preparation method thereof

    CN110364361A