An electronic grade industrial silica-based chromatographic filler and its preparation method and application
By treating silica gel with acid and combining deionized water cleaning and alcohol washing steps, the problem of poor metal ion adsorption effect of silica gel in liquid crystal materials is solved, achieving efficient metal ion removal and cost reduction, and is suitable for industrial applications.
Patent Information
- Application Number
- CN202211325150.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-27
AI Technical Summary
Existing silica gel has poor adsorption effect when removing metal ions from liquid crystal materials, and conventional modification treatment methods are complex and costly, which limits its use in industrial applications.
By acid treatment of silica gel, acid ions are used to form salts with surface metal ions and dissolved, thereby reducing the metal content. The preparation process is simplified by using sulfuric acid, hydrochloric acid, nitric acid and other acids for treatment, combined with deionized water cleaning and alcohol washing steps. .
It significantly improves the metal ion removal rate of silica gel, reduces production costs, simplifies the preparation process, is suitable for industrial production, and retains the surface and pore structure of the original silica gel.
Smart Images

Figure CN115634675B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silica gel preparation, and in particular to an electronic-grade industrial silica-based chromatographic filler and a preparation method and application thereof. Background Art
[0002] Liquid crystal, also known as mesomorphic state, is an intermediate state between three-dimensional ordered solid crystals and irregular liquids. It has both the fluidity of liquid and certain arrangement characteristics similar to crystals. The intermolecular forces of liquid crystals are weaker than those of solids. Under the action of electric fields, magnetic fields, heat and other energies, the arrangement of liquid crystal molecules will change, causing changes in its optical, electrical and magnetic physical properties. For example, under the action of an electric field, the arrangement of liquid crystal molecules will change, thus affecting its optical properties. This is called the photoelectric effect. Using the photoelectric effect of liquid crystals, liquid crystals have been applied to many fields, especially in the field of flat panel displays. With the rapid development of the information industry, the requirements of liquid crystal display devices for liquid crystal materials are constantly increasing.
[0003] According to the needs of display technology, the compounds or compositions that make up liquid crystal materials should have higher resistivity, higher charge retention rate, higher thermal stability and photoelectric stability, lower viscosity, etc. However, a small amount of metal ions usually remain in the liquid crystal during the preparation process. The presence of these metal ions will reduce the resistivity of the liquid crystal material, thereby reducing the charge retention rate, which limits the application of the liquid crystal material.
[0004] Silica gel is a highly active adsorption material. Silica gel is an amorphous substance with a chemical formula of mSiO2·nH2O. It is insoluble in water and any solvent, non-toxic and tasteless, and has stable chemical properties. Silica gel is usually used as a silica-based chromatographic filler. It can effectively adsorb and remove polar impurities in liquid crystals, but for metal ions in liquid crystals, silica gel removes them through intermolecular forces (van der Waals forces), and often has the problem of poor adsorption effect on metal ions. Conventionally, in order to improve the adsorption effect of silica gel on metal ions, the surface of silica gel is modified. For example, the silica gel disclosed in the silica gel double-layer surface treatment technology is first surface bonded with orthosilicate, and then further hydrolyzed for modification. Although this method improves the adsorption effect of silica gel on metal ions, it has the defects of complex preparation process and high cost of raw materials for modification. Summary of the invention
[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the prior art in improving the adsorption effect of silica gel on metal ions, such as complex preparation and high cost, thereby providing an electronic-grade industrial silica-based chromatographic filler and a preparation method and application thereof to solve the above problems.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme:
[0007] The invention discloses a method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising: subjecting silica gel to acid treatment to obtain the filler.
[0008] Preferably, the acid is at least one of sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid, hydrobromic acid, hydroiodic acid, iodic acid, periodic acid, and perchloric acid.
[0009] Preferably, the concentration of the acid is above 3%, for example 3%, 5%, 8%, 10%, 15%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, etc.
[0010] Preferably, the acid concentration adjusting agent is at least one of water, ethanol, methanol, propanol and isopropanol.
[0011] Preferably, the temperature of the acid treatment is below 100°C.
[0012] Preferably, the acid treatment lasts for less than 30 hours.
[0013] Preferably, deionized water is used for washing after the acid treatment.
[0014] Preferably, after the deionized water is washed to neutrality, the mixture is washed with alcohol for 2-3 times and then dried.
[0015] Preferably, the acid treatment process can be carried out in a reactor; the reactor is made of a material that is non-reactive with acid, such as an enamel reactor, a glass reactor or a fiberglass-reinforced plastic reactor.
[0016] The present invention also provides an electronic-grade industrial silica-based chromatographic filler, which is prepared by the above-mentioned method for preparing an electronic-grade industrial silica-based chromatographic filler.
[0017] The invention also provides an application of an electronic-grade industrial silicon dioxide-based chromatographic filler in adsorbing metal ions in liquid crystal materials.
[0018] The technical solution of the present invention has the following advantages:
[0019] The present invention provides a method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising: treating silica gel with acid to obtain the filler. The acid forms rust on the surface of the silica gel, and the rusted metal can combine with acid radical ions to form corresponding salts and dissolve in water, thereby achieving the effect of reducing the metal content on the surface;
[0020] In addition, the silica gel prepared by the present invention can not only retain the surface and pore structure of the original silica gel, but also greatly reduce the metal ion content in the original silica gel. It is also verified that the silica gel after the treatment can significantly improve the removal rate of metal ions in the liquid crystal after being used for liquid crystal adsorption treatment, and the effect is remarkable. The preparation of the silica gel in the present invention is simpler, the production cost is low, and it is more conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 It is a curve chart showing the change of the iron and sodium metal ion contents in the electronic-grade industrial silica-based chromatographic fillers prepared in Examples 1-9 of the present invention with the concentration of sulfuric acid. DETAILED DESCRIPTION
[0023] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0024] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the art can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially. The concentrations not clearly specified in the present invention are all mass concentrations.
[0025] Example 1
[0026] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0027] First, add 900 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 100 ml of concentrated sulfuric acid (concentration of concentrated sulfuric acid is 98%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100 ° C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0028] Example 2
[0029] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0030] First, add 800 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 200 ml of concentrated sulfuric acid (concentration of concentrated sulfuric acid is 98%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100 ° C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0031] Example 3
[0032] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0033] First, add 700 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 300 ml of concentrated sulfuric acid (concentration of concentrated sulfuric acid is 98%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100 ° C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0034] Example 4
[0035] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0036] First, add 600 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 400 ml of concentrated sulfuric acid (concentration of concentrated sulfuric acid is 98%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100 ° C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0037] Example 5
[0038] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0039] First, add 500 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 500 ml of concentrated sulfuric acid (concentration of concentrated sulfuric acid is 98%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100 ° C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0040] Example 6
[0041] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0042] First, add 400 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 600 ml of concentrated sulfuric acid (concentration of concentrated sulfuric acid is 98%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100 ° C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0043] Example 7
[0044] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0045] First, add 300 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 700 ml of concentrated sulfuric acid (concentration of concentrated sulfuric acid is 98%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100 ° C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0046] Example 8
[0047] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0048] First, add 200 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 800 ml of concentrated sulfuric acid (concentration of concentrated sulfuric acid is 98%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100 ° C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0049] Example 9
[0050] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0051] First, add 100 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 900 ml of concentrated sulfuric acid (concentration of concentrated sulfuric acid is 98%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100 ° C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0052] Example 10
[0053] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0054] First, add 900 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 100 ml of sulfuric acid solution (the concentration of the sulfuric acid solution is 30%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100°C for 4 hours, cool to room temperature, and then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0055] Embodiment 11
[0056] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0057] First, add 900 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 100 ml of concentrated hydrochloric acid (the concentration of concentrated hydrochloric acid is 36%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100°C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0058] Example 12
[0059] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0060] First, add 500 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 500 ml of concentrated nitric acid (the concentration of concentrated nitric acid is 62%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100°C for 4 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0061] Example 13
[0062] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0063] First, add 500 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 500 ml of concentrated hydrochloric acid (the concentration of concentrated hydrochloric acid is 36%), and then add 100 g of silica gel. After stirring and refluxing for dehydration at 25°C for 30 hours, adjust to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0064] Embodiment 14
[0065] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0066] First, add 500 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 500 ml of concentrated hydrochloric acid (the concentration of concentrated hydrochloric acid is 36%), and then add 100 g of silica gel. After stirring and refluxing for dehydration at 10°C for 25 hours, adjust to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0067] Embodiment 15
[0068] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0069] First, add 500 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 500 ml of concentrated hydrochloric acid (the concentration of concentrated hydrochloric acid is 36%), and then add 100 g of silica gel. After stirring and refluxing for dehydration at 30°C for 20 hours, adjust to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0070] Example 16
[0071] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0072] First, add 500 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 500 ml of concentrated hydrochloric acid (concentration of concentrated hydrochloric acid is 36%), and then add 100 g of silica gel. After stirring and reflux dehydration at 50°C for 15 hours, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0073] Embodiment 17
[0074] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0075] First, add 500 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 500 ml of concentrated hydrochloric acid (concentration of concentrated hydrochloric acid is 36%), and then add 100 g of silica gel. After stirring and reflux dehydration at 70°C for 10 hours, cool to room temperature, and then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0076] Embodiment 18
[0077] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0078] First, add 500 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 500 ml of concentrated hydrochloric acid (the concentration of concentrated hydrochloric acid is 36%), and then add 100 g of silica gel. After stirring and reflux dehydration at 90°C for 5 hours, cool to room temperature, and then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0079] Embodiment 19
[0080] A method for preparing an electronic-grade industrial silica-based chromatographic filler, comprising:
[0081] First, add 500 ml of water to a four-necked flask with a volume of 1000 ml, then slowly add 500 ml of concentrated hydrochloric acid (the concentration of concentrated hydrochloric acid is 36%), and then add 100 g of silica gel. After stirring and reflux dehydration at 100°C for 1 hour, cool to room temperature, then filter with a sand core funnel, wash with deionized water until neutral, and then wash with 300 ml of methanol 2-3 times, and then dry to obtain electronic grade industrial silica-based chromatographic filler.
[0082] Comparative Example 1
[0083] The electronic grade industrial silica-based chromatographic filler in this comparative example is the silica gel in Example 1 that has not been acid-treated.
[0084] Test Example 1
[0085] The sodium iron content was detected using the electronic grade industrial silica substrate chromatographic filler prepared in Examples 1-9 and Comparative Example 1. The test results are shown in Tables 1 and Figure 1 shown.
[0086] Table 1
[0087]
[0088]
[0089] According to Table 1 and Figure 1 It can be seen from the data that the acid treatment method of the present invention can effectively purify silica gel and significantly reduce the sodium iron content in the silica gel.
[0090] Test Example 2
[0091] The silica gel of the embodiment and comparative example 1 was used to test the metal ion adsorption capacity of the liquid crystal material, and the test process was as follows:
[0092] 10 kg of liquid crystal material was added into a sealed stirring vessel, 800 g of silica gel was added, and the mixture was stirred and adsorbed at 40° C. for 6 hours. The mixture was filtered to obtain a purified liquid crystal material. The purified liquid crystal material was tested for metal ions. The test results of Example 10 and Comparative Example 1 are shown in Tables 2 and 3.
[0093] Table 2
[0094]
[0095]
[0096] Table 3
[0097]
[0098] The lower the content of metal ions in the silica gel, the better the adsorption effect on the metal ions in the liquid crystal. Compared with the silica gel in Example 10, the silica gel products prepared in other examples have better metal ion purification effects on the liquid crystal material. Compared with the untreated silica gel in Comparative Example 1, the silica gel prepared in the embodiment of the present invention has higher purity and better adsorption effect on the metal ions in the liquid crystal material.
[0099] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. An application of an electronic grade industrial silica-based chromatographic filler in adsorbing metal ions in liquid crystal materials, characterized in that: The liquid crystal material is a black and white monomer liquid crystal, and the preparation method of the electronic-grade industrial silica-based chromatographic filler comprises: acid-treating silica gel to obtain the filler; The concentration of the acid is ≥ 70%.
2. The use according to claim 1, characterized in that: The acid is at least one of sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid, hydrobromic acid, hydroiodic acid, iodic acid, periodic acid, and perchloric acid.
3. The use according to claim 1 or 2, characterized in that: The acid concentration adjusting agent is at least one of water, ethanol, methanol, propanol and isopropanol.
4. The use according to claim 1 or 2, characterized in that: The temperature of the acid treatment is 100° C. or lower.
5. The use according to claim 1 or 2, characterized in that: The duration of the acid treatment is less than 30 hours.
6. The use according to claim 1 or 2, characterized in that: After the acid treatment, deionized water is used for washing.
7. The use according to claim 6, characterized in that: After the deionized water is washed to neutrality, the mixture is washed with alcohol for 2-3 times and then dried.
Citation Information
Patent Citations
Method for preparing high-purity mono-disperse silicon dioxide hydrosol
CN101973557A
Manufacture method for liquid crystal materials
CN102070384A
Terminal estergroup silicagel high-effect hydrophobic chromatographic stuffing and synthesis
CN1092426A
Preparation method of high-purity porous spherical silica gel filler
CN109865497A
Method and device for producing high-purity electronic-grade propylene glycol methyl ether acetate
CN114702385A