Mixed antisolvents for the fabrication of perovskite solar cells and their applications
By using a mixed antisolvent of ethyl acetate and sodium dehydroacetate, the environmental pollution problem caused by antisolvents was solved, and the stability of the perovskite layer and the performance of the battery were improved by passivating defects, thus realizing the preparation of green and environmentally friendly perovskite solar cells.
Patent Information
- Application Number
- CN202211488640.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-11-25
AI Technical Summary
The antisolvents used in existing technologies are harmful to the environment and health, and the defects of perovskite films lead to low battery efficiency and instability, making it difficult to promote them on a large scale.
A perovskite layer was prepared by using ethyl acetate and sodium dehydroacetate as a mixed antisolvent through gradient spin coating and annealing, which passivated defects and optimized the interface, resulting in a smooth and stable perovskite layer.
This improves the photoelectric performance and stability of perovskite solar cells, making them suitable for large-scale application and avoiding environmental pollution.
Smart Images

Figure CN115643781B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of perovskite solar cell technology, and specifically relates to a mixed antisolvent for preparing perovskite solar cells and its application. Background Technology
[0002] The formation process of perovskite nuclei is a key factor determining the surface morphology and coverage of thin films, and controlling the crystallization nucleation process is crucial for preparing high-quality perovskite thin films. According to classical crystallization nucleation theory, reducing solution solubility or increasing solution concentration can effectively improve the nucleation rate and density.
[0003] Therefore, in the preparation of perovskite thin films, in order to improve the nucleation rate and density of the films, the nucleation rate of perovskite thin films is generally improved by introducing antisolvents to reduce the solubility of the solution or by accelerating the evaporation of solvents to increase the solution concentration.
[0004] Patent CN110718632 A discloses a method for preparing a large-area perovskite layer, including the following steps: coating a perovskite precursor solution onto a substrate to form a perovskite precursor layer; A mixed antisolvent was added to the perovskite precursor layer, and the perovskite layer was obtained by annealing. The mixed antisolvent is a mixture of solvent A and solvent B. Solvent A is selected from any one of toluene, chlorobenzene, dichloromethane, ethyl acetate, anisole, and diethyl ether. Solvent B is selected from any one of toluene, chlorobenzene, dichloromethane, ethyl acetate, anisole, and monohydric alcohols with 3-6 carbon atoms. Solvent A and solvent B are different. Solvent A accounts for 10%-90% of the volume of the mixed antisolvent.
[0005] However, using toxic solvents such as chloroform or chlorobenzene as antisolvents would have a significant impact on the environment and human health, hindering large-scale promotion and application.
[0006] Besides, defects in the perovskite bulk phase and on its surface are one of the main factors leading to low battery efficiency and device instability. This is because perovskite films prepared by solution methods are typically polycrystalline, meaning that the perovskite film structure is disordered, resulting in grain boundary defects and crystal defects. Although these defects are shallow, they can form charge recombination centers, affecting charge transport and thus reducing battery efficiency; furthermore, these defects can adsorb oxygen and water vapor, causing perovskite degradation and affecting battery stability. Therefore, effective passivation of the perovskite surface is crucial for improving battery efficiency and stability.
[0007] The literature (Nat.Commun.2018,DOI: 10.1038 / s41467-018-05583-w) discloses that introducing excess PbI2 into the perovskite layer reduces the defect concentration in the film. The PbI2-rich perovskite film has more ordered grains, and the residual PbI2 surrounds the perovskite grains, thereby effectively improving the charge transport of the perovskite solar cell, eliminating hysteresis, and effectively suppressing charge recombination.
[0008] For example, CN112467038 A discloses a method for passivating a perovskite thin film layer, which involves preparing a perovskite precursor solution; pretreating a substrate composed of a conductive glass / electron transport layer; coating the perovskite precursor solution onto the substrate and heating it to generate a perovskite thin film layer; and further passivating and modifying the perovskite thin film layer with a fluorosulfonate to form a fluorosulfonate-modified perovskite thin film layer. The fluorosulfonate ions stabilize I-, preventing I- from escaping.
[0009] Such methods still suffer from the problem that most of the passivation solvents used are toxic, and the potential environmental pollution and adverse effects on human health limit their large-scale industrial promotion and application.
[0010] In summary, how to provide an antisolvent that can accelerate crystal growth, passivate defects on the surface of perovskite layers, and is environmentally friendly is a technical problem that urgently needs to be solved. Summary of the Invention
[0011] The purpose of this invention is to overcome the shortcomings of the prior art and provide a mixed antisolvent for preparing perovskite solar cells and its application, which can passivate defects on the surface of the perovskite layer while avoiding environmental pollution.
[0012] This invention provides a mixed antisolvent for preparing perovskite solar cells, comprising ethyl acetate and sodium dehydroacetate.
[0013] Furthermore, the concentration of the sodium dehydroacetate is 1-5 mg / ml.
[0014] This invention provides a method for preparing a perovskite layer, comprising the following steps: preparing a perovskite precursor solution; During the spin-coating process of the perovskite precursor solution, a mixed antisolvent, comprising ethyl acetate and sodium dehydroacetate, is added dropwise; annealing treatment is then performed to obtain the perovskite layer.
[0015] Furthermore, the concentration of the perovskite precursor solution is 0.6–1.4 M.
[0016] Furthermore, during the spin-coating process of the perovskite precursor solution, the addition of the mixed antisolvent includes the following steps: First, spin-coat the perovskite precursor solution at a speed of 1500 rpm / min - 2500 rpm / min for 10 s - 20 s, then spin-coat the perovskite precursor solution at a speed of 4000 rpm / min - 5000 rpm / min for 30 s - 40 s, and add 400 μL - 600 μL of the mixed antisolvent 5 - 10 s before the end of spin-coating.
[0017] Furthermore, the annealing process includes the following steps: annealing at 100℃-120℃ for 10 min - 20 min.
[0018] The present invention provides a perovskite solar cell comprising, from bottom to top, a transparent substrate layer, a bottom electrode layer, a hole transport layer, an electron transport layer and a top electrode layer, wherein a perovskite layer prepared as described above is disposed between the hole transport layer and the electron transport layer.
[0019] Furthermore, the perovskite layer is CsFAMAPbI3; the electron transport layer is SnO2.
[0020] Furthermore, the thickness of the perovskite layer is 400–600 nm.
[0021] This invention provides a method for preparing a perovskite solar cell as described in any one of the above-mentioned methods, comprising the following steps: Obtain a transparent conductive substrate; Deposit a bottom electrode layer on a transparent conductive substrate; A hole transport layer was prepared on the bottom electrode layer by spin coating. A perovskite precursor solution and a mixed antisolvent are prepared, wherein the mixed antisolvent includes ethyl acetate and sodium dehydroacetate; the mixed antisolvent is added dropwise during the spin-coating of the perovskite precursor solution onto the hole transport layer; and the perovskite layer is obtained after annealing. An electron transport layer was prepared on a perovskite layer by spin coating. A top electrode layer is formed by vapor deposition on the electron transport layer.
[0022] By adopting the above technical solution, this invention, as an example, has the following advantages and positive effects compared with the prior art: By using ethyl acetate in the mixed antisolvent to passivate defects and sodium dehydroacetate to optimize the interface, the mixed antisolvent can accelerate crystal growth, passivate defects on the perovskite layer surface, and optimize the electron transport performance of the electron transport layer. Furthermore, the mixed antisolvent avoids environmental pollution, making it environmentally friendly.
[0023] The perovskite layer prepared using a mixed antisolvent has a smooth and uniform surface, good stability and repeatability, and fewer defects, thereby improving the photoelectric performance and stability of perovskite solar cells including this perovskite layer.
[0024] The preparation process is easy to implement and environmentally friendly, making it suitable for large-scale promotion and application. Attached Figure Description
[0025] Figure 1 A performance test data table for perovskite solar cells provided in embodiments of the present invention.
[0026] Figure 2 This is a schematic diagram of the current density-voltage curve of a perovskite solar cell provided in an embodiment of the present invention.
[0027] Figure 3(A) is a SEM image of the perovskite surface without the addition of mixed antisolvents provided in the embodiment of the present invention.
[0028] Figure 3(B) is a SEM image of the perovskite surface with added mixed antisolvent provided in the embodiment of the present invention. Detailed Implementation
[0029] The technical solutions disclosed in this invention will be described in detail below with reference to specific embodiments.
[0030] Techniques and methods known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques and methods should be considered part of the specification. In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values.
[0031] In the description of this invention, it should be understood that the terms "upper" and "lower" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting this invention.
[0032] This invention provides a mixed antisolvent for preparing perovskite solar cells, comprising ethyl acetate and sodium dehydroacetate.
[0033] In this process, ethyl acetate is used as the solvent, and the concentration of sodium dehydroacetate as the solute is 1-5 mg / ml.
[0034] This invention provides a method for preparing a perovskite layer, comprising the following steps: A perovskite precursor solution is prepared; during the spin-coating process of the perovskite precursor solution, a mixed antisolvent is added dropwise, the mixed antisolvent comprising ethyl acetate and sodium dehydroacetate, wherein ethyl acetate is used to passivate surface defects of the perovskite layer; annealing treatment is performed to obtain the perovskite layer.
[0035] Preferably, the concentration of the perovskite precursor solution is 0.6–1.4 M.
[0036] During the spin-coating process of the perovskite precursor solution, the mixed antisolvent is added dropwise using gradient spin-coating, specifically including the following steps: First, spin-coat the perovskite precursor solution at a speed of 1500 rpm / min - 2500 rpm / min for 10 s - 20 s, then spin-coat the perovskite precursor solution at a speed of 4000 rpm / min - 5000 rpm / min for 30 s - 40 s, and 5 - 10 s before the end of spin-coating, add 400 μL - 600 μL of mixed antisolvent.
[0037] The annealing process includes the following steps: annealing at 100℃-120℃ for 10 min - 20 min.
[0038] The present invention provides a perovskite solar cell comprising, from bottom to top, a transparent substrate layer, a bottom electrode layer, a hole transport layer, an electron transport layer and a top electrode layer, wherein a perovskite layer as prepared above is disposed between the hole transport layer and the electron transport layer.
[0039] Preferably, the perovskite layer is CsFAMAPbI3; and the electron transport layer is SnO2.
[0040] Preferably, the thickness of the perovskite layer is 400 nm to 600 nm.
[0041] Sodium dehydroacetate in the perovskite layer acts at the interface between the perovskite layer and the electron transport layer. Sodium dehydroacetate provides charged functional groups, maximizing dipole formation at the interface and effectively controlling the work function, improving boundary properties, and influencing the electronic energy state of the surrounding environment. This reduces the perovskite / ETL interface resistance, thereby accelerating efficient electron extraction and transport. Simultaneously, because ethyl acetate passivates defects in the perovskite film, the number of grain boundaries in the perovskite film decreases, which also slows down the carrier recombination rate.
[0042] This invention provides a method for preparing a perovskite solar cell as described in any one of the above-mentioned methods, comprising the following steps: Obtain a transparent conductive substrate.
[0043] The transparent substrate can be glass or a transparent polymer. The transparent polymer can be polyetherimide (PEI), polyethylene terephthalate (PET), or polyethylene naphthalate (PEN). The transparent substrate can also be a flexible mesh silver substrate.
[0044] A bottom electrode layer can be deposited on a transparent substrate, which can be achieved by magnetron sputtering.
[0045] The bottom electrode layer includes, but is not limited to, ITO, FTO, AZO, PEDOT, metal nanowires, or graphene.
[0046] A hole transport layer is fabricated on the bottom electrode layer: the hole transport layer can be fabricated on the bottom electrode layer by spin coating, spraying, electron beam evaporation deposition, printing, magnetron sputtering, or slot coating techniques. The hole transport layer material includes, but is not limited to, any one of CuI, CuSCN, NiOx, PEDOT:PSS, Spiro-OMeTAD, PTAA, and P3HT.
[0047] A perovskite precursor solution and a mixed antisolvent were prepared: the mixed antisolvent consisted of ethyl acetate and sodium dehydroacetate; the mixed antisolvent was added dropwise during spin-coating of the perovskite precursor solution onto the hole transport layer, using the gradient spin-coating method mentioned above. The perovskite layer was obtained after annealing. The annealing process included annealing at 100 °C–120 °C for 10–20 min.
[0048] Preferably, the perovskite layer is CsFAMAPbI3.
[0049] An electron transport layer was prepared on a perovskite layer by spin coating.
[0050] Preferably, the electron transport layer is a SnO2 electron transport layer.
[0051] A top electrode layer is formed by vapor deposition on the electron transport layer.
[0052] The top electrode layer includes, but is not limited to, one or more of the following: metal electrodes (including Ag, Al, Cu, and Au), carbon electrodes, and metal oxide electrodes. Example 1
[0053] In this embodiment, the transparent substrate is a PET substrate, and an ITO conductive layer is deposited on the PET substrate by magnetron sputtering.
[0054] A PTAA hole transport layer with a thickness of 20 nm was obtained by slit coating on an ITO conductive layer.
[0055] In this embodiment, the perovskite is a CsFAMAPbI3 system, and the solvent is DMF & DMSO.
[0056] The perovskite precursor solution for preparing the perovskite layer includes the following steps: S1: Weigh 135.88 mg FAI, 25.44 mg MAI, and 461 mg PbI2 and dissolve them in 950 μL of a mixed solution of DMF and DMSO in a ratio of approximately 4:1. Stir overnight at 60°C. S2: Then weigh 259.81 mg CsI and dissolve it in 1 ml DMSO. Stir at 70°C for about 2 to 3 hours to obtain a CsI solution. Then take 50 μL from the CsI solution and add it to the solution prepared in S1 to mix into a 1 ml 1 M precursor solution.
[0057] S3: Gradient spin coating is used. The first stage is spin coating at 2500 rpm / min for 10 s, and the second stage is spin coating at 5000 rpm / min for 30 s. 5 s before the end of spin coating, 500 μl of green mixed solvent is added. The green mixed solvent is ethyl acetate as solvent and sodium dehydroacetate at 1 mg / ml.
[0058] S4: Anneal at 100℃ for 20 min. Obtain a perovskite layer with a thickness of 500 nm.
[0059] An electron transport layer of SnO2 was spin-coated onto the perovskite layer at 3000 rpm for 30 seconds, followed by annealing at 120°C for 30 minutes. The thickness of the electron transport layer was approximately 30 nm.
[0060] A 100 nm thick Ag electrode was obtained by vapor deposition on the electron transport layer. Example 2
[0061] In this embodiment, the transparent substrate is a PET substrate, and an ITO conductive layer is deposited on the PET substrate by magnetron sputtering.
[0062] A 20 nm thick PEDOT:PSS hole transport layer was deposited on the ITO conductive layer by electron beam evaporation.
[0063] In this embodiment, the perovskite is a CsFAMAPbI3 system, and the solvent is DMF & DMSO.
[0064] The preparation steps of the perovskite precursor solution for the perovskite layer can be referred to in Example 1, and the concentration of the obtained perovskite precursor solution is 0.6M.
[0065] Gradient spin coating was used. The first stage was spin coating at 2000 rpm / min for 20 s, and the second stage was spin coating at 4000 rpm / min for 50 s. 5 s before the end of spin coating, 400 μL of green mixed solvent was added. The green mixed solvent was ethyl acetate with sodium dehydroacetate at 3 mg / mL.
[0066] Annealing at 120℃ for 10 min yielded a perovskite layer with a thickness of 400 nm.
[0067] An electron transport layer of SnO2 was spin-coated onto the perovskite layer at 3000 rpm for 30 seconds, followed by annealing at 120°C for 30 minutes. The thickness of the electron transport layer was approximately 30 nm.
[0068] A 120 nm thick Au electrode was obtained by vapor deposition on the electron transport layer. Example 3
[0069] In this embodiment, the transparent substrate is a PET substrate, and an ITO conductive layer is deposited on the PET substrate by magnetron sputtering.
[0070] A 50 nm thick Spiro-MeOTAD layer was coated on the ITO conductive layer as a hole transport layer.
[0071] In this embodiment, the perovskite is a CsFAMAPbI3 system, and the solvent is DMF & DMSO.
[0072] The preparation steps of the perovskite precursor solution for the perovskite layer can be referred to in Example 1, and the concentration of the obtained perovskite precursor solution is 1.4M.
[0073] Gradient spin coating was used. The first stage was spin coating at 1500 rpm / min for 20 s, and the second stage was spin coating at 4000 rpm / min for 40 s. 10 s before the end of spin coating, 600 μL of green mixed solvent was added. The green mixed solvent was ethyl acetate with sodium dehydroacetate at a concentration of 5 mg / mL.
[0074] Annealing at 110℃ for 12 min yielded a perovskite layer with a thickness of 600 nm.
[0075] An electron transport layer of SnO2 was spin-coated onto the perovskite layer at 3000 rpm for 30 seconds, followed by annealing at 120°C for 30 minutes. The thickness of the electron transport layer was approximately 30 nm.
[0076] A 100 nm thick Ag electrode was obtained by vapor deposition on the electron transport layer.
[0077] Figure 1 Performance test data for perovskite solar cells prepared using mixed antisolvents in Examples 1-3 are presented. Figure 2 The current density-voltage curves of perovskite solar cells prepared by mixing antisolvents in Examples 1-3 are shown. The results indicate that the use of sodium dehydroacetate can optimize and improve the performance of perovskite solar cells, and the concentration of sodium dehydroacetate affects the optimization effect.
[0078] In several tests, the battery achieved the highest current density and optimal efficiency when the concentration of sodium dehydroacetate was 3 mg / ml.
[0079] Figure 3(A) shows the perovskite surface without the added antisolvent, while Figure 3(B) shows the perovskite surface with the added antisolvent. The comparison shows that the perovskite surface with the added antisolvent is smoother, more uniform, and has fewer defects. The antisolvent can passivate defects on the perovskite surface.
[0080] Within the scope of this disclosure, terms such as “comprising” should be interpreted by default as inclusive or open-ended, rather than exclusive or closed, unless expressly defined as such. All technical, scientific, or other terms shall be interpreted as understood by one of those skilled in the art, unless defined as such. Public terms found in dictionaries should not be interpreted in an overly idealistic or impractical manner in the context of the relevant technical documentation, unless expressly defined as such in this disclosure.
[0081] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0082] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A method for preparing a perovskite layer, characterized in that, Includes the following steps: Prepare perovskite precursor solution; During the spin-coating of the perovskite precursor solution, a mixed antisolvent, comprising ethyl acetate and sodium dehydroacetate, is added dropwise; an annealing treatment is then performed to obtain the perovskite layer, wherein the concentration of sodium dehydroacetate is 1-5 mg / ml. The addition of the mixed antisolvent includes the following steps: First, spin-coat the perovskite precursor solution at a speed of 1500 rpm / min-2500 rpm / min for 10 s-20 s, then spin-coat the perovskite precursor solution at a speed of 4000 rpm / min-5000 rpm / min for 30 s-40 s, and add 400 ul-600 ul of the mixed antisolvent 5-10 s before the end of spin-coating; The annealing process includes the following steps: annealing at 100℃-120℃ for 10min-20min.
2. The method for preparing the perovskite layer according to claim 1, characterized in that: The concentration of the perovskite precursor solution is 0.6–1.4 M.
3. A perovskite solar cell, comprising, from bottom to top, a transparent substrate layer, a bottom electrode layer, a hole transport layer, an electron transport layer, and a top electrode layer, characterized in that: A perovskite layer prepared according to any one of claims 1 to 2 is provided between the hole transport layer and the electron transport layer.
4. The perovskite solar cell according to claim 3, characterized in that: The perovskite layer is CsFAMAPbI3; the electron transport layer is SnO2.
5. The method for preparing a perovskite solar cell according to claim 3, characterized in that: The thickness of the perovskite layer is 400–600 nm.
6. A method for preparing a perovskite solar cell as described in any one of claims 3-5, characterized in that, Includes the following steps: Obtain a transparent conductive substrate; Deposit a bottom electrode layer on a transparent conductive substrate; A hole transport layer is fabricated on the bottom electrode layer; Prepare a perovskite precursor solution and a mixed antisolvent, wherein the mixed antisolvent comprises ethyl acetate and sodium dehydroacetate; The mixed antisolvent is added dropwise during the spin coating of the perovskite precursor solution onto the hole transport layer, and the perovskite layer is obtained after annealing. An electron transport layer was prepared on a perovskite layer by spin coating. A top electrode layer is formed by vapor deposition on the electron transport layer.
Citation Information
Patent Citations
Method for preparing large-area perovskite layer and perovskite solar cell
CN110718632A
High-efficiency perovskite solar cell prepared by use of green mixed anti-solvent and preparation method
CN109638168A