Polyurethane modified acrylate and vinyl acetate-acrylic copolymer emulsion adhesive thereof

By copolymerizing polyurethane-modified acrylate with vinyl acetate and combining acetalized polyvinyl alcohol, the water resistance and stability of the acetic acrylic emulsion is solved, and a high bond strength and antibacteriality of the acrylic copolymer emulsion adhesive is achieved. , improves the mechanical properties of the adhesive film.

CN118931432APending Publication Date: 2024-11-12MEGABOND HUANGSHAN ADHESIVE
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411226730.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult for acrylic copolymer emulsion to have good water resistance and stability. The existing improved methods such as the introduction of silicone have problems with phase separation, which affects the stability of the emulsion.

Method used

Polyurethane modified acrylate is used to copolymerize with vinyl acetate, and acetal-acrylic emulsion adhesive with high bond strength, antibacterial properties and good water resistance is prepared by acetalizing polyvinyl alcohol and a specific reactant.

Benefits of technology

The stability, water resistance and bonding strength of the adhesive are improved, and the antibacterial effect is enhanced through the quaternary ammonium salt structure, improving the mechanical properties of the adhesive film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024827180000101
    Figure BDA0005024827180000101
  • Figure BDA0005024827180000111
    Figure BDA0005024827180000111
Patent Text Reader

Abstract

The invention discloses a polyurethane modified acrylic ester and vinyl acetate-acrylic copolymer emulsion adhesive and a preparation method thereof, and belongs to the technical field of adhesives, the adhesive comprises the following raw materials by weight: 18-25 parts of acetalated polyvinyl alcohol; 180 to 200 parts of vinyl acetate; 40 to 50 parts of butyl acrylate; 10 to 15 parts of polyurethane modified acrylic ester; 0.5 to 0.8 part of sodium acetate; 4-5 parts of an emulsifier; 0.5 to 0.75 part of an initiator; 240 to 260 parts of water; the preparation method comprises the following steps: stirring and mixing the raw materials according to the ratio at a proper temperature, preparing polyurethane modified acrylate by taking hydroxyethyl acrylate, toluene-2, 4-diisocyanate and N, N, N-trimethyl-2-hydroxyhexadecyl ammonium chloride as raw materials, and applying the polyurethane modified acrylate to the preparation of the emulsion adhesive, so that the obtained adhesive has the characteristics of high stability, high viscosity, high viscosity, high viscosity and the like. The adhesive has the advantages of high adhesive strength, good water resistance and high adhesive strength, and has good antibacterial property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives, and in particular relates to a polyurethane-modified acrylate and an acetic acid-acrylic copolymer emulsion adhesive. Background Art

[0002] Among the interior and exterior wall emulsion products synthesized by emulsion polymerization, vinyl acetate acrylic emulsion synthesized with vinyl acetate as the main raw material plays a very important role both in the industrial field and in the scientific research field. Compared with the traditional styrene acrylic or pure acrylic emulsion, vinyl acetate acrylic emulsion is deeply favored by the majority of paint manufacturers and consumers due to its excellent construction performance, less odor, unique rheological properties, and high film-forming stability.

[0003] However, vinyl acetate emulsion also has its own insurmountable defects. The main reason is that the raw material vinyl acetate is highly water-soluble, resulting in the water resistance of vinyl acetate emulsion is not very ideal. To address this problem, silicone is currently introduced into vinyl acetate emulsion to improve it. For example, Chinese patent No. CN107722881A discloses a method for preparing vinyl acetate emulsion adhesive. In the process of emulsion preparation, silane coupling agent KH-550 is introduced to improve the water resistance of the emulsion. However, there are still some problems: for example, due to the presence of water in the emulsion polymerization, hydrolysis and condensation reactions of alkoxy groups occur, which seriously affects the progress of the emulsion polymerization reaction; due to the huge gap between organic siloxane and acrylate in molecular structure and polarity, different degrees of phase separation will occur due to compatibility problems, resulting in poor emulsion stability. Summary of the invention

[0004] The object of the present invention is to provide a polyurethane-modified acrylate and an acrylate copolymer emulsion adhesive thereof, so as to solve the problem that the existing acrylate copolymer emulsion is difficult to have both good water resistance and stability.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A polyurethane-modified acrylate and its acetic acid-acrylic copolymer emulsion adhesive, comprising the following raw materials in parts by weight:

[0007] 18-25 parts of acetalized polyvinyl alcohol;

[0008] 180-200 parts of vinyl acetate;

[0009] Butyl acrylate 40-50 parts;

[0010] 10-15 parts of polyurethane modified acrylate;

[0011] Sodium acetate 0.5-0.8 parts;

[0012] 4-5 parts of emulsifier;

[0013] Initiator 0.5-0.75 parts;

[0014] 240-260 parts of water.

[0015] Furthermore, the polyurethane modified acrylate is obtained by a two-step reaction of hydroxyethyl acrylate, toluene-2,4-diisocyanate and N,N,N-trimethyl-2-hydroxyhexadecyl ammonium chloride.

[0016] Furthermore, the preparation method of the polyurethane-modified acrylate comprises the following steps:

[0017] Add toluene-2,4-diisocyanate to a flask, and dropwise add a hydroxyethyl acrylate solution containing an inhibitor at 35°C with stirring. After the addition is complete, keep the temperature for reaction for 1 hour, then raise the temperature to 40°C for reaction for 3 hours, then raise the temperature to 70°C, and dropwise add a tetrahydrofuran solution of N,N,N-trimethyl-2-hydroxyhexadecylammonium chloride with stirring. After the addition is complete, keep the temperature for reaction for 1.7-2 hours, and finally remove the tetrahydrofuran by rotary evaporation to obtain polyurethane-modified acrylate.

[0018] Furthermore, the dripping rate is 4-6 mL / min.

[0019] Furthermore, the molar ratio of toluene-2,4-diisocyanate, hydroxyethyl acrylate, and N,N,N-trimethyl-2-hydroxyhexadecyl ammonium chloride is 1:1:1.

[0020] Furthermore, in the hydroxyethyl acrylate solution containing the polymerization inhibitor, the mass of the polymerization inhibitor is 0.5% of the mass of the hydroxyethyl acrylate.

[0021] Furthermore, the amount of tetrahydrofuran in the tetrahydrofuran solution of N,N,N-trimethyl-2-hydroxyhexadecylammonium chloride is 8-12 times the mass of N,N,N-trimethyl-2-hydroxyhexadecylammonium chloride.

[0022] Furthermore, the polymerization inhibitor is one or more of 2,6-di-tert-butyl-p-methylphenol, p-hydroxyanisole and hydroquinone.

[0023] Furthermore, the acetalized polyvinyl alcohol is obtained by acetalizing polyvinyl alcohol and 3,4-dihydroxybenzaldehyde.

[0024] Furthermore, the preparation method of acetalized polyvinyl alcohol comprises the following steps:

[0025] Add polyvinyl alcohol and dimethyl sulfoxide into a flask, heat to 80-90°C with stirring, continue stirring for 2 hours, add p-toluenesulfonic acid and 3,4-dihydroxybenzaldehyde, keep warm and stir for 6-9 hours. After the reaction is completed, pour the reaction product into a container filled with distilled water, and a white solid precipitates. Filter it, wash the filter cake with deionized water and then vacuum dry it at 50°C to constant weight to obtain acetalized polyvinyl alcohol.

[0026] Furthermore, the mass ratio of polyvinyl alcohol to 3,4-dihydroxybenzaldehyde is 15:5.2-6.0.

[0027] Furthermore, the amount of p-toluenesulfonic acid used is 2-4% of the total mass of polyvinyl alcohol and 3,4-dihydroxybenzaldehyde.

[0028] Furthermore, the usage ratio of polyvinyl alcohol and dimethyl sulfoxide is 15 g:100 mL.

[0029] Furthermore, the polyvinyl alcohol was PVA1799, obtained from Chengdu Kelong Chemical Reagent Factory, analytical grade.

[0030] Furthermore, the initiator is ammonium persulfate.

[0031] Furthermore, the emulsifier is lauryl alcohol polyoxyethylene ether.

[0032] A method for preparing a polyurethane-modified acrylate and an acetic acid-acrylic copolymer emulsion adhesive, comprising the following steps:

[0033] Add 80% of the total water mass into the reactor, add acetalized polyvinyl alcohol under stirring, heat to 90°C and keep warm for reaction for 1 hour, then cool to 78°C, add sodium acetate aqueous solution and emulsifier, stir for 20 minutes, add initiator aqueous solution of 40% of the total initiator aqueous solution mass, the initiator aqueous solution is mixed with the initiator and the remaining water, then add mixed monomer dropwise, add 10% of the remaining initiator aqueous solution mass every 1 hour during the dropwise addition of the mixed monomer, control the dropping time to 6 hours, after the dropwise addition is completed, keep warm for reaction for 15 minutes, heat to 85°C and continue to react for 1 hour, cool to 40°C, and obtain polyurethane modified acrylate and its acrylate copolymer emulsion adhesive.

[0034] Furthermore, the mass ratio of sodium acetate to water in the aqueous solution of sodium acetate is 1:3.

[0035] Furthermore, the mixed monomer is formed by mixing vinyl acetate, butyl acrylate and polyurethane-modified acrylate.

[0036] Beneficial effects of the present invention:

[0037] 1. The present invention uses hydroxyethyl acrylate, toluene-2,4-diisocyanate and N,N,N-trimethyl-2-hydroxyhexadecyl ammonium chloride as raw materials, and prepares polyurethane-modified acrylate containing polyurethane units, acrylate structures, quaternary ammonium salt structures and alkyl long chains through the reaction between -NCO and -OH, and uses it as a new monomer material to copolymerize with vinyl acetate and butyl acrylate to prepare vinyl acetate-acrylic copolymer emulsion adhesive, which has the advantages of high stability, good water resistance, high bonding strength, and good antibacterial properties. The specific analysis is as follows:

[0038] The rigid benzene ring structure and high bonding strength urethane bond in the polyurethane-modified acrylate give the adhesive good film cohesive strength. The long alkyl chain has excellent flexibility and low polarity, which is beneficial to improving the mechanical properties and water resistance of the adhesive film. The quaternary ammonium salt structure gives the film a good antibacterial effect.

[0039] 2. In the present invention, acetalized polyvinyl alcohol is obtained by acetalization reaction of polyvinyl alcohol and 3,4-dihydroxybenzaldehyde, and the acetalized polyvinyl alcohol is used to replace conventional polyvinyl alcohol as a protective colloid. Since the symmetry of the polyvinyl alcohol molecule is destroyed, the interaction between the hydroxyl group and the H2O molecule on the molecule is reduced, the number of hydrophilic groups is reduced, and the emulsion stability and water resistance are improved. In addition, the acetalized polyvinyl alcohol in the present invention also contains a catechol structure, which increases the bonding interaction between the adhesive and the substrate surface, further improving the bonding strength of the adhesive.

[0040] 3. The present invention accurately controls the proportion of acetalized polyvinyl alcohol in the adhesive raw material because experiments show that too low or too high an acetalized polyvinyl alcohol dosage will affect the stability of the adhesive.

[0041] 4. The present invention strictly controls the ratio of polyvinyl alcohol and 3,4-dihydroxybenzaldehyde in the preparation process of acetalized polyvinyl alcohol. If the amount of 3,4-dihydroxybenzaldehyde is too low, the acetalization degree of polyvinyl alcohol is low, and it is difficult to significantly improve the emulsion stability, water resistance and bonding strength of the adhesive. If the amount of 3,4-dihydroxybenzaldehyde is too high, the emulsification effect of polyvinyl alcohol will be weakened, resulting in poor stability of the adhesive. DETAILED DESCRIPTION

[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] In the following examples and comparative examples, polyvinyl alcohol is PVA1799, obtained from Chengdu Kelong Chemical Reagent Factory, analytical grade.

[0044] Example 1

[0045] A polyurethane-modified acrylate, the preparation method comprising the following steps:

[0046] Add 41.80g of toluene-2,4-diisocyanate to the flask, and add a mixed solution consisting of 27.87g of hydroxyethyl acrylate and 0.14g of 2,6-di-tert-butyl-p-methylphenol dropwise at 35°C and 150rpm with stirring. The drop rate is 4mL / min. After the dropwise addition is completed, keep the temperature for reaction for 1h, then heat to 40°C for reaction for 3h, then heat to 70°C, and add a mixed solution consisting of 80g of N,N,N-trimethyl-2-hydroxyhexadecyl ammonium chloride and 640g of tetrahydrofuran dropwise with stirring. The drop rate is 4mL / min. After the dropwise addition is completed, keep the temperature for reaction for 1.7h, and remove tetrahydrofuran by rotary evaporation to obtain polyurethane-modified acrylate.

[0047] Example 2

[0048] A polyurethane-modified acrylate, the preparation method comprising the following steps:

[0049] Add 41.80g of toluene-2,4-diisocyanate to the flask, and add a mixed solution consisting of 27.87g of hydroxyethyl acrylate and 0.14g of p-hydroxyanisole dropwise at 35°C and 150rpm with stirring. The drop rate is 6mL / min. After the dropwise addition is completed, keep warm for reaction for 1h, then heat to 40°C for reaction for 3h, then heat to 70°C, and add a mixed solution consisting of 80g of N,N,N-trimethyl-2-hydroxyhexadecylammonium chloride and 960g of tetrahydrofuran dropwise with stirring. The drop rate is 6mL / min. After the dropwise addition is completed, keep warm for reaction for 2h, and remove tetrahydrofuran by rotary evaporation to obtain polyurethane-modified acrylate.

[0050] Comparative Example 1

[0051] A polyurethane-modified acrylate, the preparation method is different from that in Example 1, except that the step of "adding dropwise a mixed solution of 80 g of N,N,N-trimethyl-2-hydroxyhexadecyl ammonium chloride and 640 g of tetrahydrofuran while stirring" in Example 1 is replaced by "adding dropwise 31.26 g of 2-ethylhexanol while stirring", and the remaining raw materials, processes and parameters are the same as in Example 1.

[0052] Example 3

[0053] A polyurethane-modified acrylate and its acetic acid-acrylic copolymer emulsion adhesive, comprising the following raw materials in parts by weight:

[0054] Acetalized polyvinyl alcohol 18 g;

[0055] Vinyl acetate 200g;

[0056] Butyl acrylate 50g;

[0057] 15 g of the polyurethane-modified acrylate of Example 1;

[0058] Sodium acetate 0.8 g;

[0059] 5g of polyoxyethylene lauryl ether;

[0060] Ammonium persulfate 0.75 g;

[0061] 260g deionized water.

[0062] The preparation method of acetalized polyvinyl alcohol comprises the following steps:

[0063] Add 15g of polyvinyl alcohol and 100mL of dimethyl sulfoxide into a flask, heat to 80°C with stirring, continue stirring for 2h, add 0.4g of p-toluenesulfonic acid and 5.2g of 3,4-dihydroxybenzaldehyde, keep warm and stir for 6h. After the reaction is completed, pour the reaction product into a container filled with distilled water, and a white solid precipitates. Filter it, wash the filter cake with deionized water, and vacuum dry it at 50°C to constant weight to obtain acetalized polyvinyl alcohol.

[0064] The preparation method of the polyurethane-modified acrylate and its vinyl acetate-acrylic copolymer emulsion adhesive comprises the following steps:

[0065] Add 80% of the total deionized water mass to the reactor, add acetalized polyvinyl alcohol under stirring, heat to 90°C and keep warm for reaction for 1h, then cool to 78°C, add sodium acetate aqueous solution and lauryl alcohol polyoxyethylene ether, the mass ratio of sodium acetate to deionized water in the sodium acetate aqueous solution is 1:3, stir for 20min, add 40% of the total ammonium persulfate aqueous solution mass of ammonium persulfate aqueous solution, the ammonium persulfate aqueous solution is mixed with ammonium persulfate and the remaining deionized water, then add mixed monomer dropwise, add 10% of the remaining ammonium persulfate aqueous solution mass every 1h during the dropwise addition of the mixed monomer, control the dropwise addition time to 6h, after the dropwise addition is completed, keep warm for reaction for 15min, heat to 85°C and continue to react for 1h, cool to 40°C, and obtain polyurethane modified acrylate and its acrylate copolymer emulsion adhesive.

[0066] The mixed monomer is obtained by mixing vinyl acetate, butyl acrylate and polyurethane-modified acrylate in a mixer at 300 rpm for 30 minutes.

[0067] Example 4

[0068] A polyurethane-modified acrylate and its acetic acid-acrylic copolymer emulsion adhesive, comprising the following raw materials in parts by weight:

[0069] Acetalized polyvinyl alcohol 21.5 g;

[0070] Vinyl acetate 190g;

[0071] Butyl acrylate 45g;

[0072] 12.5 g of the polyurethane-modified acrylate of Example 2;

[0073] Sodium acetate 0.7 g;

[0074] 4.5 g of polyoxyethylene lauryl ether;

[0075] Ammonium persulfate 0.65 g;

[0076] 250g deionized water.

[0077] The preparation method of acetalized polyvinyl alcohol comprises the following steps:

[0078] Add 15g of polyvinyl alcohol and 100mL of dimethyl sulfoxide into a flask, heat to 85°C with stirring, continue stirring for 2h, add 0.6g of p-toluenesulfonic acid and 5.6g of 3,4-dihydroxybenzaldehyde, keep warm and stir for 8h. After the reaction is completed, pour the reaction product into a container filled with distilled water, and a white solid precipitates. Filter it, wash the filter cake with deionized water, and vacuum dry it at 50°C to constant weight to obtain acetalized polyvinyl alcohol.

[0079] The preparation method of the above-mentioned polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive is the same as that in Example 3.

[0080] Example 5

[0081] A polyurethane-modified acrylate and its acetic acid-acrylic copolymer emulsion adhesive, comprising the following raw materials in parts by weight:

[0082] Acetalized polyvinyl alcohol 25g;

[0083] Vinyl acetate 180g;

[0084] Butyl acrylate 40g;

[0085] 10 g of the polyurethane-modified acrylate of Example 2;

[0086] Sodium acetate 0.5g;

[0087] 4g of lauryl polyoxyethylene ether;

[0088] Ammonium persulfate 0.5 g;

[0089] 240g deionized water.

[0090] The preparation method of acetalized polyvinyl alcohol comprises the following steps:

[0091] Add 15g of polyvinyl alcohol and 100mL of dimethyl sulfoxide into a flask, heat to 90°C with stirring, continue stirring for 2h, add 0.8g of p-toluenesulfonic acid and 6.0g of 3,4-dihydroxybenzaldehyde, keep warm and stir for 9h. After the reaction is completed, pour the reaction product into a container filled with distilled water, and a white solid precipitates. Filter it, wash the filter cake with deionized water, and vacuum dry it at 50°C to constant weight to obtain acetalized polyvinyl alcohol.

[0092] The preparation method of the above-mentioned polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive is the same as that in Example 3.

[0093] Comparative Example 2

[0094] A polyurethane-modified acrylate and its vinyl acetate-acrylic copolymer emulsion adhesive, compared with Example 3, the difference is that the polyurethane-modified acrylate in Example 3 is replaced by the product prepared in Comparative Example 1, and the other raw materials, processes and parameters are the same as Example 3.

[0095] Comparative Example 3

[0096] A polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive, compared with Example 3, the difference is that the acetalized polyvinyl alcohol in Example 3 is replaced by polyvinyl alcohol, and the other raw materials, processes and parameters are the same as Example 3.

[0097] Comparative Example 4

[0098] A polyurethane-modified acrylate and its vinyl acetate-acrylic copolymer emulsion adhesive, compared with Example 3, the difference is that the "5.2g of 3,4-dihydroxybenzaldehyde" in Example 3 is modified to "5.1g of 3,4-dihydroxybenzaldehyde", and the other raw materials, processes and parameters are the same as Example 3.

[0099] Comparative Example 5

[0100] A polyurethane-modified acrylate and its vinyl acetate-acrylic copolymer emulsion adhesive, compared with Example 3, the difference is that the "6.0g of 3,4-dihydroxybenzaldehyde" in Example 3 is modified to "6.1g of 3,4-dihydroxybenzaldehyde", and the other raw materials, processes and parameters are the same as Example 3.

[0101] Comparative Example 6

[0102] A polyurethane-modified acrylate and its acetal copolymer emulsion adhesive, compared with Example 3, the difference is that the "acetalized polyvinyl alcohol 18g" in Example 3 is changed to "acetalized polyvinyl alcohol 17g", and the other raw materials, processes and parameters are the same as Example 3.

[0103] Comparative Example 7

[0104] A polyurethane-modified acrylate and its acetal-acrylic copolymer emulsion adhesive, compared with Example 5, the difference is that the "acetalized polyvinyl alcohol 25g" in Example 5 is changed to "acetalized polyvinyl alcohol 26g", and the other raw materials, processes and parameters are the same as Example 5.

[0105] The adhesives obtained from Examples 3 to 5 and Comparative Examples 2 to 7 were subjected to performance tests, and the testing process was as follows:

[0106] (1) Freeze-thaw stability

[0107] Place each group of adhesives in a -15°C freezer, freeze for 24 hours, take them out and thaw them at 25±0.5°C for 1.5 hours, then use a glass rod to take samples for coating. If the coating film is delicate and smooth, it indicates that the emulsion has good freeze-thaw stability, otherwise the freeze-thaw stability is poor.

[0108] (2) Bonding strength

[0109] According to the standard test of HG / T 2727-2010, poplar wood is selected as the material of the sample, the bonding area is 15mm×20mm, and the glue amount is 150g / m 2 , apply each group of adhesives to the two bonding surfaces of the sample, overlap and bond the test pieces, apply a pressure of 1MPa to the bonding surface, and keep it for 24h, the temperature is (25±2℃), the relative humidity is 40-60%, and after the pressure is released, place it in this environment for 48h, and test it with a universal mechanical testing machine. The shear strength σ is:

[0110] σ=P / A; where σ is shear strength, MPa, and A is the bonding area of ​​the specimen, mm 2 , P is the maximum load when the bonding area is damaged, N.

[0111] (3) Water absorption

[0112] Each group of adhesives was coated on a glass plate, left at room temperature for 24 hours, then the film was removed and cut into 10cm x 10cm samples, weighed as M1, and then placed in deionized water for 48 hours, and finally the sample was taken out and the surface moisture was wiped dry and weighed as M2, and three parallel measurements were made, and the results were averaged. The water absorption rate P is: P = (M2-M1) / M1×100%.

[0113] (4) Antibacterial properties

[0114] The antibacterial test was carried out by the inhibition ring method, using Staphylococcus aureus and Escherichia coli as the test bacteria. The bacteria were cultured and diluted to 106 / mL of bacterial liquid was then smeared on an agar plate and cultured in a 37°C incubator for 12 h. Each group of adhesives was made into a sample with a diameter of 5 mm and a thickness of 1 mm. The samples were immersed in a 10wt% ethanol solution for 24 h. After drying, the samples were placed on agar plates respectively and cultured in an incubator for 12 h. The diameter of the antibacterial ring was measured after taking out.

[0115] The test results are shown in Table 1:

[0116] Table 1

[0117]

[0118]

[0119] It can be seen from the data recorded in Table 1 that the polyurethane-modified acrylate and its vinyl acetate-acrylic copolymer emulsion adhesive prepared by the present invention have better comprehensive performance and have greater promotion value in the market.

[0120] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0121] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive, characterized in that: In parts by weight, the following raw materials are included: 18-25 parts of acetalized polyvinyl alcohol; 180-200 parts of vinyl acetate; Butyl acrylate 40-50 parts; 10-15 parts of polyurethane modified acrylate; Sodium acetate 0.5-0.8 parts; 4-5 parts of emulsifier; Initiator 0.5-0.75 parts; 240-260 parts of water.

2. The polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive according to claim 1, characterized in that: The polyurethane modified acrylate is obtained by two-step reaction of hydroxyethyl acrylate, toluene-2,4-diisocyanate and N,N,N-trimethyl-2-hydroxyhexadecyl ammonium chloride.

3. The polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive according to claim 1, characterized in that: Preparation method of polyurethane modified acrylate, The following steps are involved: At 35°C, add a solution of hydroxyethyl acrylate containing an inhibitor dropwise into toluene-2,4-diisocyanate with stirring. After the addition is complete, keep the temperature for reaction for 1 hour, then raise the temperature to 40°C for reaction for 3 hours, then raise the temperature to 70°C, add a solution of N,N,N-trimethyl-2-hydroxyhexadecylammonium chloride in tetrahydrofuran dropwise with stirring. After the addition is complete, keep the temperature for reaction for 1.7-2 hours, and rotary evaporate to obtain polyurethane-modified acrylate.

4. The polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive according to claim 3, characterized in that: The molar ratio of toluene-2,4-diisocyanate, hydroxyethyl acrylate, and N,N,N-trimethyl-2-hydroxyhexadecyl ammonium chloride is 1:1:

1.

5. The polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive according to claim 1, characterized in that: Acetalized polyvinyl alcohol is obtained by acetalization reaction of polyvinyl alcohol and 3,4-dihydroxybenzaldehyde.

6. The polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive according to claim 1, characterized in that: The preparation method of acetalized polyvinyl alcohol comprises the following steps: Mix polyvinyl alcohol and dimethyl sulfoxide, raise the temperature to 80-90°C while stirring, continue stirring for 2 hours, add p-toluenesulfonic acid and 3,4-dihydroxybenzaldehyde, keep warm and stir to react for 6-9 hours, pour the reaction product into a container filled with distilled water, filter with suction, wash and dry the filter cake to obtain acetalized polyvinyl alcohol.

7. The polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive according to claim 6, characterized in that: The mass ratio of polyvinyl alcohol to 3,4-dihydroxybenzaldehyde is 15:5.2-6.

0.

8. The polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive according to claim 6, characterized in that: The amount of p-toluenesulfonic acid used is 2-4% of the total mass of polyvinyl alcohol and 3,4-dihydroxybenzaldehyde.

9. A method for preparing the polyurethane-modified acrylate and its vinyl acetate-acrylic copolymer emulsion adhesive according to any one of claims 1 to 8, characterized in that: The following steps are involved: Add 80% of the total water mass into the reactor, add acetalized polyvinyl alcohol under stirring, heat to 90°C and keep warm for reaction for 1 hour, then cool to 78°C, add sodium acetate aqueous solution and emulsifier, stir for 20 minutes, add initiator aqueous solution of 40% of the total initiator aqueous solution mass, the initiator aqueous solution is mixed with the initiator and the remaining water, then add mixed monomer dropwise, add 10% of the remaining initiator aqueous solution mass every 1 hour during the dropwise addition of the mixed monomer, control the dropping time to 6 hours, after the dropwise addition is completed, keep warm for reaction for 15 minutes, heat to 85°C and continue to react for 1 hour, cool to 40°C, and obtain polyurethane modified acrylate and its acrylate copolymer emulsion adhesive.

10. The method for preparing a polyurethane-modified acrylate and its acetate-acrylic copolymer emulsion adhesive according to claim 9, characterized in that: The mass ratio of sodium acetate to water in the sodium acetate aqueous solution is 1:3, and the mixed monomer is prepared by mixing vinyl acetate, butyl acrylate, and polyurethane-modified acrylate.

Citation Information

Cited By

  • Binder for diaphragm, preparation method of binder, modified diaphragm and battery

    CN121022312A

  • A binder for a separator, a method for preparing the same, a modified separator, and a battery

    CN121022312B