A silver-containing antibacterial agent and its preparation method and application

By doping silver ions into hydrotalcite and combining it with organic ligands, an efficient silver-containing antibacterial agent is prepared, which solves the problems of complicated processes and insufficient biocompatibility of silver-based antibacterial agents in the existing technology, and achieves efficient sterilization and Wound healing effect.

CN115645547BActive Publication Date: 2024-10-11ZHEJIANG TOP-MEDICAL MEDICAL DRESSING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211340441.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-10-11
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

The preparation process of existing silver-based antibacterial agents is complicated, the silver content is low, and it is easy to cause allergic reactions in users, making it difficult to balance biocompatibility and efficient antibacterial properties.

Method used

Using a combination of silver-containing hydrotalcite and organic ligands, silver ions are doped into the hydrotalcite through a reaction to prepare a stable and efficient silver-containing antibacterial agent for use in the design of antibacterial dressings.

Benefits of technology

It achieves efficient killing of infectious bacteria, promotes wound healing, reduces side effects, and provides a simple production method and good biocompatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115645547B_ABST
    Figure CN115645547B_ABST
Patent Text Reader

Abstract

The present invention discloses a silver-containing antibacterial agent and a preparation method and application thereof, and belongs to the technical field of pharmaceutical preparations. The preparation method comprises the following steps: adding a magnesium source and an aluminum source to water to obtain a solution A; mixing and reacting the solution A and an alkali solution, and then adding a silver source solution thereto to react, and after the reaction is completed, centrifuging and drying to obtain a silver-containing hydrotalcite; dispersing the obtained silver-containing hydrotalcite into an organic ligand solution, stirring and reacting, and obtaining a silver-containing antibacterial agent. The antibacterial agent prepared by the method has good biocompatibility and effective antibacterial properties, and can promote skin tissue repair; in the preparation process of the present invention, silver ions are doped into the hydrotalcite, which not only increases the broad spectrum of antibacterial properties, but also increases biocompatibility. By combining the silver-containing hydrotalcite with the organic ligand, the effect of the silver-containing antibacterial agent can be efficiently improved, providing a new design strategy for a new antibacterial dressing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of pharmaceutical preparations, and in particular to a silver-containing antibacterial agent and a preparation method and application thereof. Background Art

[0002] Optimal management of infected wounds involves preventing infection while also promoting the natural wound healing process. A common method for preventing infection in infected wounds is the use of silver because of its effective antimicrobial properties. Silver is a highly effective antimicrobial agent, and the antimicrobial mechanisms of metallic silver ions reported so far are as follows: 1) Silver ions inhibit the synthesis of adenosine triphosphate (ATP) synthase by binding to the cell wall; 2) Silver ions enter cells and bind to DNA, causing DNA denaturation; 3) Silver ions hinder the microbial respiratory chain in the cytochrome oxidase and nicotinamide adenine dinucleotide succinate dehydrogenase regions. Silver is coated or combined with polymers to produce silver dressings, which can cover the wound area to provide protection while maintaining a moist environment to allow wound healing and reduce the risk of infection. However, poorly designed silver antimicrobial agents in dressings can easily reduce their antimicrobial properties, and it is often difficult to achieve compatibility between biocompatibility and high-efficiency antimicrobial properties.

[0003] At present, most of the silver-based antibacterial agents are prepared by ion exchange method, with low silver content, and some products need to be sintered at high temperature and then crushed into micro powder, which has complex manufacturing process and high cost; and silver-based antibacterial agents constructed by loading process, such as silver-containing antibacterial agents constructed by biomacromolecule chitosan and its derivatives, in which silver ions are easily released quickly and in large quantities, which may cause allergic reactions in users. Therefore, the present invention provides a silver-containing antibacterial agent prepared by using hydrotalcite with good biocompatibility. Summary of the invention

[0004] The purpose of the present invention is to provide a silver-containing antibacterial agent and a preparation method and application thereof to solve the problems existing in the above-mentioned prior art. The present invention utilizes the combination of silver-containing hydrotalcite and organic ligands to prepare a stable and efficient silver-containing antibacterial agent, providing a new design strategy for a new antibacterial dressing.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] The present invention provides a method for preparing a silver-containing antibacterial agent, comprising the following steps:

[0007] (1) Preparing silver-containing hydrotalcite: adding a magnesium source and an aluminum source into water to obtain a solution A; mixing the solution A with an alkali solution for reaction, and then adding a silver source solution thereto for reaction. After the reaction is completed, centrifuging and drying to obtain the silver-containing hydrotalcite;

[0008] (2) dispersing the silver-containing hydrotalcite obtained in step (1) into an organic ligand solution, stirring and reacting, and obtaining a silver-containing antibacterial agent.

[0009] Furthermore, in step (1), the uniform hydroxyl lattice and different crystal plane orientations of the hydrotalcite highly disperse the catalytically active silver atoms and tightly anchor them on the high-energy crystal planes of the hydrotalcite, thereby exposing more active silver particles.

[0010] Furthermore, in step (1), the magnesium source is any one or more of magnesium chloride, magnesium sulfate and magnesium nitrate; the aluminum source is any one or more of aluminum chloride, aluminum sulfate and aluminum nitrate; the silver source is any one or more of silver nitrate, silver thiosulfate and silver sulfate; and the alkali solution includes sodium hydroxide.

[0011] Furthermore, in step (1), the molar ratio of the magnesium source, the aluminum source, the alkali solution and the silver source is (6-12): (4-12): (1-8): (0.5-2.5).

[0012] Furthermore, in step (1), the mixing reaction time is 15-55 min; the reaction time is 1.5-3 h.

[0013] Furthermore, in step (2), the organic ligand solution includes a sodium carboxyphenyl borate solution; the concentration of the sodium carboxyphenyl borate solution is 0.1-0.3 mg / mL; the stirring reaction time is 1-3 hours; and the concentration of the silver-containing antibacterial agent is 0.2-2.6 mg / mL.

[0014] The present invention also provides a silver-containing antibacterial agent obtained according to the above preparation method.

[0015] The present invention also provides an application of the silver-containing antibacterial agent in preparing a dressing for repairing an infectious wound.

[0016] Furthermore, the silver-containing antibacterial agent achieves the effect of repairing the infected wound surface by killing infectious bacteria at the wound surface, inhibiting the expression of pro-inflammatory factors and promoting the formation of collagen fibers.

[0017] Furthermore, the infectious bacteria include Staphylococcus aureus and Escherichia coli; the pro-inflammatory factors include IL-6 and TNF-α.

[0018] The present invention discloses the following technical effects:

[0019] 1. The present invention utilizes functional organic ligands to mix with silver-containing hydrotalcite, and silver ions are doped into the hydrotalcite during the preparation process, which not only increases the broad spectrum of antibacterial properties, but also increases biocompatibility. The combination of silver-containing hydrotalcite and organic ligands can effectively improve the effect of silver-containing antibacterial agents, providing a new design strategy for new antibacterial dressings.

[0020] 2. The method of the present invention is a novel method for directly preparing a silver-containing antibacterial agent. The method is simple, has low fixed investment, short production cycle, and is easy for large-scale production.

[0021] 3. The silver-containing antibacterial agent prepared by the present invention can effectively kill Gram bacteria, and can kill bacteria at the infectious wound surface, effectively promoting wound healing. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 is the XRD spectrum of the silver-containing hydrotalcite in the present invention;

[0024] Figure 2 The figure is a diagram showing the cytotoxicity and antibacterial effect of the silver-containing antibacterial agent of the present invention;

[0025] Figure 3 The silver-containing antibacterial agent of the present invention is used for repairing the size of bacterial-infected wounds in rats and the hematoxylin-eosin (H&E) staining diagram;

[0026] Figure 4 The bacterial plating diagram and the statistical results of bacterial survival rate in the wound tissue area of ​​the rat model of the present invention;

[0027] Figure 5 This is a Masson's Trichrome staining restoration diagram of the silver-containing antibacterial agent of the present invention used for bacterially infected wounds in rats;

[0028] Figure 6 The silver-containing antibacterial agent of the present invention is used for immunofluorescence images of IL-6 and TNF-α in the repair tissue of bacterial-infected wounds in rats;

[0029] Figure 7 These are H&E images of the liver and kidney of each group of rats after the silver-containing antibacterial agent of the present invention was used for repairing infected wounds in rats. DETAILED DESCRIPTION

[0030] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0031] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0032] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0033] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0034] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0035] Example 1 Preparation method of a silver-containing antibacterial agent

[0036] The following steps are involved:

[0037] (1) A magnesium source: magnesium chloride (0.6 M) and an aluminum source: aluminum chloride (1.0 M) were added to 0.5 L of distilled water, and a uniform solution A was obtained by mechanical stirring. 0.8 M of alkali (sodium hydroxide) was added to 1 L of distilled water and a uniform solution B was obtained by mechanical stirring. Solution A and solution B were mixed and reacted for 15 minutes, and then 0.2 L of an aqueous solution of silver nitrate (0.05 M) was added thereto, and the mixture was reacted for 2 hours, followed by centrifugation and drying to obtain silver-containing hydrotalcite powder (Ag-LDH).

[0038] (2) A sodium carboxyphenylborate aqueous solution (0.1 mg / mL) (SCPB) was prepared to obtain solution C, and the silver-containing hydrotalcite was dispersed therein. The mixture was stirred for reaction for 2 hours to obtain the silver-containing antibacterial agent SCPB@Ag-LDH (0.4 mg / mL).

[0039] Example 2 Preparation method of a silver-containing antibacterial agent

[0040] The following steps are involved:

[0041] (1) A magnesium source: magnesium sulfate (0.6 M) and an aluminum source: aluminum nitrate (0.2 M) were added to 0.5 L of distilled water, and a uniform solution A was obtained by mechanical stirring. A base (sodium hydroxide) 0.1 M was added to 1 L of distilled water and a uniform solution B was obtained by mechanical stirring. Solution A and solution B were mixed and reacted for 30 minutes, and then 0.2 L of silver nitrate (0.03 M) solution was added thereto. The mixture was reacted for 1 hour, and then centrifuged and dried to obtain silver-containing hydrotalcite powder (Ag-LDH).

[0042] (2) A sodium carboxyphenylborate aqueous solution (0.1 mg / mL) (SCPB) was prepared to obtain solution C, and the silver-containing hydrotalcite was dispersed therein. The reaction was stirred for 3 hours to obtain the silver-containing antibacterial agent SCPB@Ag-LDH (0.2 mg / mL).

[0043] Example 3

[0044] The following steps are involved:

[0045] (1) A magnesium source: magnesium nitrate (0.3 M) and an aluminum source: aluminum sulfate (6.0 M) were added to 0.5 L of distilled water, and a uniform solution A was obtained by mechanical stirring. 0.3 M of alkali (sodium hydroxide) was added to 1 L of distilled water and a uniform solution B was obtained by mechanical stirring. Solution A and solution B were mixed and reacted for 55 minutes, and then 0.2 L of silver nitrate (0.01 M) solution was added thereto. The mixture was reacted for 3 hours, and then centrifuged and dried to obtain silver-containing hydrotalcite powder (Ag-LDH).

[0046] (2) A sodium carboxyphenylborate aqueous solution (0.3 mg / mL) (SCPB) was prepared to obtain solution C, and the silver-containing hydrotalcite was dispersed therein. The reaction was stirred for 1 hour to obtain the silver-containing antibacterial agent SCPB@Ag-LDH (2.6 mg / mL).

[0047] Comparative Example 1

[0048] A magnesium source: magnesium chloride (0.6 M) and an aluminum source: aluminum chloride (1.0 M) were added to 0.5 L of distilled water, and a uniform solution A was obtained by mechanical stirring. 0.8 M of alkali (sodium hydroxide) was added to 1 L of distilled water, and a uniform solution B was obtained by mechanical stirring. Solution A and solution B were mixed, reacted for 15 minutes, and then centrifuged and dried to obtain hydrotalcite powder (LDH).

[0049] Comparative Example 2

[0050] The only difference from Example 1 is that step (2) is omitted and silver-containing hydrotalcite powder (Ag-LDH) is obtained according to step (1).

[0051] Effect verification

[0052] 1. XRD patterns of silver-containing antibacterial agents

[0053] The silver-containing hydrotalcite powder (Ag-LDH) prepared in Example 1 was tested by X-ray powder diffractometer. The results are as follows: Figure 1 The results showed that the characteristic peaks of hydrotalcite were consistent with those of silver oxide, which confirmed that the silver-containing hydrotalcite was successfully constructed in the present invention.

[0054] 2. Safety of silver-containing antimicrobial agents

[0055] The CCK-8 method was used to detect cell viability. Mouse fibroblasts (L929) were cultured in DMEM containing 10% fetal bovine serum and 1% penicillin-streptomycin. Mouse fibroblasts were plated at 1×10 cells per well in the presence of 5% carbon dioxide and 37°C. 4 The cells were inoculated in a 24-well plate at a density of 10 cells. After the cells were incubated for 24 h, the silver-containing antibacterial agent SCPB@Ag-LDH prepared in Example 1 and an equal amount of PBS were added to the 24-well (transwell) as a control group. After incubation with the silver-containing antibacterial agent and PBS for 1 day, the cell culture medium was replaced with 500 μL of fresh DMEM containing 10% (v / v) CCK-8 solution and incubated in the dark. After culturing for 2 h, 200 μL of the supernatant was placed in a 96-well plate, and the optical density (OD) of the culture plate solution at 450 nm was measured using a spectrophotometer.

[0056] Cell viability = OD (experimental - blank) / OD (control - blank) * 100%.

[0057] The experimental results are as follows Figure 2 As shown in the figure, the silver-containing antibacterial agent is low toxic or basically non-toxic as a whole, but with the increase of dosage, a small part of the cell activity is lost. Therefore, SCPB@Ag-LDH with a concentration of 0.2 mg / mL was selected in the subsequent experimental work.

[0058] 3. In vitro antibacterial effect of SCPB@Ag-LDH

[0059] Prepare Staphylococcus aureus (S. aureus) in TSB and Escherichia coli (E. coli) in LB. First, mix 50 μL of the stock solution with 9.95 mL of growth medium and incubate for 12 h (37°C, 250 rpm). Then centrifuge and dilute to a concentration of 10 6 CFU / mL of bacterial suspension was used to generate colonies by dilution method.

[0060] To verify the in vitro antibacterial effect of the silver-containing antibacterial agent, Staphylococcus aureus and Escherichia coli were selected as model bacteria. The SCPB@Ag-LDH prepared in Example 1 was placed in a 24-well plate. Three parallel experimental wells were added to each group. Then, 500 μL of the prepared bacterial broth was added to these centrifuge tubes and contacted with the gel for 1 hour. Then, 50 μL of the bacterial solution was taken out and dropped onto the agar plate, evenly dispersed, and incubated at 37°C for 15h-24h. The results are shown in Figure 2. Figure 2 SCPB@Ag-LDH has obvious antibacterial effect on two microorganisms (Escherichia coli and Staphylococcus aureus), basically killing all the bacteria, which proves that the silver-containing antibacterial agent SCPB@Ag-LDH prepared by the present invention has good antibacterial properties.

[0061] 4. Repair effect of SCPB@Ag-LDH on infected wounds

[0062] Experimental methods:

[0063] HE staining steps: The tissue slides are processed as follows: a. Dewaxing, dewaxing xylene I and II for 10 minutes each, and prepare coverslips in advance; b. Covering with water, 100% (I, II), 90%, 80%, 70% alcohol for 5 minutes each, and rinsing with tap water for 5 minutes × 3; c. Hematoxylin staining for 5 minutes, depending on the staining situation, the staining time can be appropriately increased or decreased, and rinsed with running water; d. Differentiation with 5% acetic acid for 1 minute, rinse with running water, add acetic acid with a pipette, and cover the tissue on the slide. After differentiation, the color becomes lighter and becomes blue. e. Blueing: Blueing liquid, which is not available in the laboratory, can also be used. f. Eosin staining for 1 minute, depending on the staining situation, the staining time can be appropriately increased or decreased, and rinsed with running water. g. Dehydration: 70%, 80%, 90%, 100% alcohol for 10 seconds each, xylene for 1 minute, and it can be dried naturally in a fume hood and then sealed, about 5 minutes. h. Apply neutral gum and seal the slide. Use a pipette to apply one drop, try to use as few drops as possible, but make sure the entire tissue is covered after pressing to avoid bubbles in the middle.

[0064] To evaluate the number of bacteria in tissues, infected tissues in each group were selected, samples were spread on nutrient agar plates, and then counted. Each group was tested in parallel with 3 groups.

[0065] Masson trichrome staining steps: a. routine dewaxing of sections to water; b. staining with prepared Weigert iron hematoxylin staining solution for 5 min-10 min; c. thorough water washing, if over-stained, hydrochloric acid alcohol differentiation; d. bluing with Masson bluing solution for 3-5 min, then water washing; e. washing with distilled water for 1 min; f. staining with Ponceau fuchsin staining solution for 5-10 min; g. preparing weak acid working solution in the ratio of distilled water: weak acid solution = 2:1 during the above operation, and washing with weak acid working solution for 1 min; h. washing with 1% phosphomolybdic acid solution for 1-2 min; i. washing with prepared weak acid working solution for 1 min; j. staining with aniline blue staining solution for 1-2 min without water washing; k. washing with prepared weak acid working solution for 1 min; l. rapid dehydration with 95% ethanol; m. dehydration with anhydrous ethanol for 3 times, 5-10 s each time; n. transparentization with xylene for 3 times, 1-2 min each time; o. sealing with neutral gum.

[0066] Immunohistochemistry experiment: a corresponding antibodies such as interleukin-6 (IL-6) and tumor necrosis factor-α (TNF-α) labeling tissue sections; b staining reaction; c microscopic observation.

[0067] The skin wound of rats was infected with Staphylococcus aureus to construct a rat skin wound model. The silver-containing antibacterial agent SCPB@Ag-LDH of Example 1, the hydrotalcite powder (LDH) of Comparative Example 1, and the silver-containing hydrotalcite powder (Ag-LDH) of Comparative Example 2 were added to the wound surface of the model, and PBS was used as a control. Figure 3 It can be seen that the skin wound areas of the treatment groups SCPB@Ag-LDH, LDH and Ag-LDH were smaller than those of the PBS group during the entire experiment. However, the wound repair speed of the SCPB@Ag-LDH group was the fastest, which may be due to the excellent bactericidal properties of the slow-release silver ions of the antibacterial agent.

[0068] In order to explore the biological mechanism of the healing process, H&E, evaluation of bacterial counts in the repaired tissue, Masson trichrome staining, and immunohistochemistry were further performed according to the above methods. Figure 3 The H&E staining results (scale: 500μm) show that on the 10th day, the dermis of the SCPB@Ag-LDH group was completely regenerated, with fewer infiltrating inflammatory cells. And from the bacterial plating data of the repaired tissue ( Figure 4 ), the number of bacteria in the tissues treated with SCPB@Ag-LDH group was significantly less than that in the other groups. Figure 5 Masson trichrome staining was used to verify the formation of collagen fibers (blue) (scale: 500 μm). The results showed that the number of collagen fibers in the SCPB@Ag-LDH group was much higher than that in the PBS group, and was also significantly higher than that in LDH and Ag-LDH. Figure 6As shown in the figure (scale bar: 500 μm), the wound surface was further stained with interleukin-6 (IL-6) and tumor necrosis factor-α (TNF-α) immunofluorescence to better understand the progress of wound healing. SCPB@Ag-LDH has the lowest expression of IL-6 and TNF-α, which confirms that the silver-containing antibacterial agent prepared by the present invention has the best inflammation regulation effect and effectively inhibits inflammation of infected wounds.

[0069] In addition, the liver and kidney of each group of rats were further analyzed. Figure 7 It can be seen (scale: 1 mm) that the organs of the rats treated with the silver-containing antibacterial agent are the same as those of the normal group, indicating that the silver-containing antibacterial agent prepared by the present invention has basically no deep-seated side effects.

[0070] In summary, these experimental results confirm that the silver-containing antibacterial agent prepared by the present invention can be used as a promising antibacterial dressing for treating bacterially infected skin wounds.

[0071] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a silver-containing antibacterial agent, characterized in that: The following steps are involved: (1) Preparing silver-containing hydrotalcite: adding a magnesium source and an aluminum source into water to obtain a solution A; mixing the solution A with an alkali solution for reaction, and then adding a silver source solution thereto for reaction. After the reaction is completed, centrifuging and drying to obtain the silver-containing hydrotalcite; (2) dispersing the silver-containing hydrotalcite obtained in step (1) into a sodium carboxyphenylborate solution, stirring and reacting, thereby obtaining a silver-containing antibacterial agent.

2. The preparation method according to claim 1, characterized in that: In step (1), the magnesium source is any one or more of magnesium chloride, magnesium sulfate and magnesium nitrate; the aluminum source is any one or more of aluminum chloride, aluminum sulfate and aluminum nitrate; the silver source is any one or more of silver nitrate, silver thiosulfate and silver sulfate; and the alkali solution includes sodium hydroxide.

3. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of the magnesium source, the aluminum source, the alkali solution and the silver source is (6-12): (4-12): (1-8): (0.5-2.5).

4. The preparation method according to claim 1, characterized in that: In step (1), the mixing reaction time is 15-55 min; the reaction time is 1.5-3 h.

5. The preparation method according to claim 1, characterized in that: In step (2), the concentration of the sodium carboxyphenylborate solution is 0.1-0.3 mg / mL; the stirring reaction time is 1-3 hours; and the concentration of the silver-containing antibacterial agent is 0.2-2.6 mg / mL.

6. A silver-containing antibacterial agent obtained according to the preparation method according to any one of claims 1 to 5.

7. Use of the silver-containing antibacterial agent according to claim 6 in preparing a dressing for repairing infectious wounds.

8. The use according to claim 7, characterized in that: The silver-containing antibacterial agent achieves the effect of repairing the infectious wound surface by killing infectious bacteria at the wound surface, inhibiting the expression of pro-inflammatory factors and promoting the formation of collagen fibers.

9. The use according to claim 8, characterized in that: The infectious bacteria include Staphylococcus aureus and Escherichia coli; the pro-inflammatory factors include IL-6 and TNF-α.