A method for preparing silicon-doped nanodiamond grains

Through the preparation method of silicon-doped nano-diamond grains, the compressed deposition system of monosilane and methane is used to fill the gaps on the diamond surface, and combined with acid etching treatment, the problem of diamond surface roughness is solved, and the nanometerization and hardness of diamond are achieved. Improved to meet the needs of precision industries such as microelectronics.

CN115652420BActive Publication Date: 2024-10-15唐合科技(内蒙古)股份有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211164359.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-23
Publication Date
2024-10-15
Estimated Expiration
2042-09-23

AI Technical Summary

Technical Problem

Existing diamond deposition methods result in rough surfaces, making it difficult to meet the needs of precision industries such as microelectronics.

Method used

The silicon-doped nano-diamond grain preparation method is used to fill the gaps on the diamond surface through a compressed deposition system of monosilane and methane, and combines low-concentration deposition with the active attraction of silicon elements to form a homogenized diamond film, which is then passed through acid Silicon-doped nanodiamond grains were obtained by liquid etching.

Benefits of technology

It effectively improves the roughness problem of diamond surface, realizes nanometerization and penetration of diamond particle size, improves hardness and toughness, and meets the needs of precision industry.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the field of diamond technology, and specifically relates to a method for preparing silicon-doped nano-diamond grains, comprising the following steps: step 1, grinding a silicon substrate; step 2, depositing diamond on the ground silicon substrate; step 3, compressing and depositing the deposited diamond for a second time; step 4, repeating step 2 and step 3 to obtain a silicon-doped diamond film; step 5, stripping the diamond film to obtain silicon-doped nano-diamond grains. The present invention solves the defects of existing diamond deposition, utilizes a compression deposition system of monosilane and methane, can form gap filling on the diamond surface, effectively improves the problem of diamond roughness, and at the same time cooperates with low-concentration deposition and active attraction of silicon element to ensure the doping and encapsulation characteristics of silicon element.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of diamonds, and in particular relates to a method for preparing silicon-doped nano-diamond grains. Background Art

[0002] Diamond has been used in various fields such as electronics, machinery, aerospace, military, optics, and medical treatment due to its high hardness, high thermal conductivity, wide optical transmittance range, and wide frequency response range. It is a very important engineering material. However, the content of natural diamond is very small and expensive, which cannot meet the needs of social production. Therefore, artificial diamonds have emerged in the market to meet the demand for diamonds. The artificial diamonds prepared by chemical vapor deposition not only have similar performance to natural diamonds, but also have low cost. However, the surface of the diamond prepared by this method is severely rough, and it is difficult to polish, which makes it difficult to meet the needs of precision industries such as microelectronics. Summary of the invention

[0003] In view of the problems in the prior art, the present invention provides a method for preparing silicon-doped nano-diamond grains, which solves the defects of the existing diamond deposition. The compressed deposition system of monosilane and methane is used to fill the gaps on the diamond surface, effectively improving the problem of diamond roughness. At the same time, low-concentration deposition and active attraction of silicon elements are combined to ensure the doping and encapsulation characteristics of silicon elements.

[0004] In order to achieve the above technical objectives, the technical solution of the present invention is:

[0005] A method for preparing silicon-doped nanodiamond grains comprises the following steps:

[0006] Step 1, grinding the silicon substrate;

[0007] Step 2, depositing diamond on the ground silicon substrate;

[0008] Step 3, performing secondary compression deposition on the deposited diamond;

[0009] Step 4, repeating steps 2 and 3 to obtain a silicon-doped diamond film;

[0010] Step 5: stripping the diamond film to obtain silicon-doped nano-diamond grains.

[0011] The grinding process in step 1 comprises the following steps: a1, grinding the silicon substrate with diamond powder to roughen the surface of the silicon substrate, wherein the diamond powder is diamond powder of different particle sizes, and the diamond powder comprises a first diamond powder with a particle size of 50-80nm and a second diamond powder with a particle size of 800-1300nm, and the mass ratio of the first diamond powder to the second diamond powder is 2:2-5; the grinding pressure is 0.7-0.9MPa, this step utilizes the different particle size distribution of diamond powder to form grinding scratches of different sizes on the surface of the silicon substrate, which can form a surface scratch structure with staggered sizes. The scratch structure is divided into large scratches and small scratches. The small scratches can be distributed in the large scratches to form a staggered structure. At the same time, based on the fact that the particle size of the first diamond powder is much smaller than that of the second diamond powder, a staggered ball-milled surface layer can be formed, which can even out the ball-milling effect of the surface, and achieve homogenization and staggering of the surface roughness structure. When the large scratches of the second diamond powder are evenly dispersed, the first diamond powder can form a secondary scratch treatment on the surface, reduce the corner buffering of the large scratch layer, and reduce the sharpness of the scratch edge; a2, the roughened silicon substrate is treated by grinding with silicon particles a3, the silicon substrate after grinding is obtained, wherein the silicon particles have a particle size of 500-1000nm, and the grinding pressure is 2-4MPa. In this step, the silicon substrate with a roughened surface is subjected to secondary grinding using the silicon particles as grinding materials. As the grinding pressure increases, the silicon particles can form a pressure-type passivation on the sharp angles based on the same material structure as the silicon substrate and the sharpness of the scratch edges of the silicon substrate, thereby reducing the angularity of the scratches. The particle size of the silicon particles is located between the first diamond powder and the second diamond powder, which can protect small scratches, and the granular structure of the silicon particles themselves can well smooth the edges of small scratches, eliminate their sharpness, and contribute to the stability of the deposited structure. a4, the silicon substrate after grinding is subjected to ultra- Acoustic cleaning, filtering and drying to obtain a clean silicon substrate, wherein the silicon substrate is ultrasonically treated with distilled water, ethanol and acetone in sequence; the ultrasonic frequency of the distilled water is 60-80kHz, the temperature is 50-60°C, and the silicon substrate is taken out and dried after the ultrasonic treatment of the distilled water is completed, and the drying temperature is 110-120°C; the ultrasonic frequency of the ethanol is 50-60kHz, the temperature is 40-50°C, and the silicon substrate is removed and dried after the ultrasonic treatment of the ethanol is completed, and the drying temperature is 80-90°C; the ultrasonic frequency of the acetone is 40-50kHz, the temperature is 10-20°C, and the silicon substrate is removed and dried after the ultrasonic treatment of the acetone is completed, and the drying temperature is 30-40°C; this step uses distilled water, ethanol and acetone to clean in sequence in combination with ultrasonic vibration. , which can completely separate and remove the impurities and residual particles on the surface, achieve rapid separation, and ensure the cleanliness of the scratches; at the same time, distilled water, ethanol and acetone all have good mutual solubility characteristics, and the step-by-step washing-drying steps can ensure the complete removal of solid particles and surface deposited impurities. At the same time, ethanol can completely remove water molecules, and acetone can also completely remove ethanol. There is basically no ethanol and water residue, and a clean silicon substrate is obtained; in the silicon substrate grinding process, diamond powder with different particle sizes is first used for pressure grinding to form scratches of varying sizes, and then the scratches are softened by using silicon particles of a medium particle size system to reduce the sharpness of the scratches. Finally, three mutually soluble solvents are used to form a gradient ultrasonic washing to obtain relatively clean scratches. .

[0012] The deposition in step 2 adopts a chemical vapor deposition method, wherein the chemical vapor deposition uses methane as a carbon source, and is combined with hydrogen and nitrogen to form a reaction gas, the gas pressure is 10-15 kPa, the microwave power is 600-800 W, the substrate temperature during deposition is 800-1000 ° C, and the deposition time is 10-20 hours. Further, in the reaction gas in the deposition, the volume proportion of methane is 5-8%, the volume proportion of hydrogen is 10-14%, and the balance is nitrogen. In this step, in the microwave plasma chemical vapor deposition equipment, methane, hydrogen and nitrogen are used to form a combined reaction gas, which, in combination with the surface concave-convex structure after grinding, can form a stable deposition effect. Moreover, the deposition is based on the fine scratches after the grinding process, which can form the miniaturization of the grains, effectively inhibit the initial growth of the grains, and at the same time, based on the limitation of its own structure, the growth of the grains is controlled, thereby forming a nanostructure. Furthermore, the grinding of the vapor deposition system and the silicon substrate provides an environmentally restricted deposition substrate, which plays a semi-directional deposition effect and effectively controls the methane deposition process. Furthermore, during the grinding process, acetone remains on the silicon substrate, which can absorb the methane of the reaction gas to form a liquid absorption, provide a nucleation prefabrication system for deposition, and help the methane deposition system. At the same time, under the deposition temperature conditions, acetone will be released to form acetone vapor, but the local methane-acetone concentration will increase slightly, which is transmitted as carbon deposition.

[0013] The compression deposition in step 3 adopts microwave vapor deposition, the reaction gas of the microwave vapor deposition is a silicon-containing reaction gas, and the silicon-containing reaction gas is a mixed gas of monosilane, methane, hydrogen and nitrogen, and the volume proportion of monosilane is 0.2-0.5%, the volume proportion of methane is 3-7%, the volume proportion of hydrogen is 13-15%, and the balance is nitrogen. The microwave power is 800-1000W, the pressure is 20-50kPa, and the pressure is gradually compressed to 60-80kPa before deposition. The temperature during deposition rises to 800-900°C within 0.5h; the deposition time is 3-6h; in this step, when the reaction gas is introduced into the microwave plasma chemical vapor deposition equipment, as the pressure gradually increases, the methane and monosilane in the gas gradually penetrate into the initially deposited diamond defects, forming a defect repair effect, At the same time, the gaseous permeability of methane and monosilane is utilized to quickly cover the defective area. When the temperature rises, monosilane decomposes in situ to form silicon material, and can form a stable connection with the diamond structure, achieving excellent silicon modification effect and permeability repair of diamond defect structure; secondly, based on the mixed structure formed by monosilane and methane, diamond itself is obtained by methane deposition, and methane is used as the raw material to bring about homogeneous penetration repair, which stabilizes and seals the silicon element and improves the fixation effect of the silicon element; in the high-temperature deposition process, monosilane will decompose and release hydrogen while converting into silicon element, effectively increasing the internal partial pressure and ensuring the stability of its own structure. At the same time, the doping of silicon element causes local activity changes, which can effectively promote the deposition of methane next to the silicon element to form a covering structure, which plays a protective role for the silicon element;

[0014] The stripping treatment in step 5 adopts acid corrosion, and the acid adopts a mixture of hydrofluoric acid and nitric acid, and the mass ratio of hydrofluoric acid to nitric acid is 2:1. In this system, hydrofluoric acid can form slow corrosion with the silicon wafer, and in this corrosion process, nitric acid can greatly improve the reaction efficiency to form fluorosilicic acid. At the same time, the structure of the diamond itself is stable, which can ensure its own stable structure, realize the dissolution of the silicon substrate, and use the solid-liquid separation method to achieve the purpose of obtaining diamond grains; at the same time, the silicon exposed on the surface of the diamond is also corroded and removed, while the silicon element wrapped in the inner layer is retained to obtain silicon-doped diamond grains with stable structure.

[0015] Furthermore, the silicon particles in a2 adopt a microporous silicon particle structure. During the grinding process, the silicon particles can sharpen the edges of the scratches, reduce the dead corners on the surface of the silicon substrate, and reduce the sharpness of the subsequently deposited diamonds; during the grinding process, the silicon particles can grind the edge of the silicon substrate into fine powder and achieve the effect of removal. Based on the fact that the subdivided material is also made of silicon, a grinding system of this grade of particles can be formed under pressure. This grinding will cause other unnecessary bumps in the scratches, resulting in unstable surface bump structure. To address this problem, the microporous silicon particle structure can form a permeable absorption of the fine powder. Based on the difference in particle size, the fine powder can be infiltrated into the micropores of the microporous silicon particle structure to achieve temporary retention. The purpose is to reduce the influence of the fine powder particles on scratches; the preparation method of the microporous silicon particle structure comprises the following steps: b1, adding sodium chloride to ethanol, adding ethyl cellulose and stirring evenly to form a slurry, spray drying to obtain composite particles, the mass ratio of sodium chloride to ethyl cellulose is 3:3-4, and the concentration of sodium chloride in ethanol is 300-500g / L, the spray drying spray speed is 5-10mL / min, and the temperature is 90-100°C; this step utilizes the gelling characteristics of sodium chloride in ethanol, which can be quickly converted into colloid particles with uniform particle size, and the colloid particles are insoluble solid small particles. At the same time, ethyl cellulose has good solubility in ethanol. b2, putting nano silicon particles into distilled water and stirring evenly, then adding the composite particles and stirring well to form a suspension, and then dry grinding and filtering to obtain prefabricated particles; the mass ratio of the nano silicon particles to the composite particles is 10:2-3, and the mass ratio of the nano silicon particles to the composite particles is 10:2-3, and the mass ratio of the nano silicon particles to the distilled water is 10:2-3, and the mass ratio of the nano silicon particles to the composite particles ... The mass is 10:1-2, the grinding temperature is 5-10°C, the pressure is 2-4MPa, the dry grinding temperature is 20-30°C, and the grinding pressure is 4-8MPa; this step uses the pressure in wet grinding to make the nano silicon particles enter the ethyl cellulose and form a uniform mixture with the ethyl cellulose, and at the same time, the packaging system of the ethyl cellulose itself is broken, resulting in the dissolution of sodium chloride. At this time, the ethyl cellulose is in an empty shell state and is formed with the nano silicon particles to form an inner and outer packaging structure, and the low particle size system of the ethyl cellulose itself achieves the purpose of dispersing and solidifying the silicon particles. The sodium chloride itself has super solubility in water and can be dissolved and removed, and the effect of stable removal is achieved by filtering;Dry grinding uses ethyl cellulose as a binder to aggregate silicon particles, and further disperses them during the grinding process. The solidification effect of grinding is used to ensure that the silicon particles connected to the same ethyl cellulose form a stable connection, and the ethyl cellulose in the structure becomes a barrier and pore-forming agent, which helps it form a porous structure; b3, pressurizing the prefabricated particles for 2-3 hours, then immersing them in an ethanol aqueous solution for ultrasonic treatment for 20-30 minutes, filtering and drying to obtain microporous silicon particles, the pressure of the pressurization treatment is 20-40MPa, the temperature is room temperature, the volume proportion of ethanol in the ethanol aqueous solution is 50-60%, and the ultrasonic frequency is 5 0-70kHz, temperature is 40-60℃; this step densifies the prefabricated particles by pressurizing, effectively improving the compactness and connectivity of the particles, and having an excellent and stable structure. At the same time, ultrasonic treatment can dissolve ethyl cellulose, and distilled water dissolves the residual sodium chloride to achieve the effect of rapid removal; this process uses sodium chloride as a support for ethyl cellulose to form an ethyl cellulose shell, and uses low-particle silicon particles in the grinding process to fill it, and cooperates with secondary grinding to form a stable connection between silicon particles and ethyl cellulose, and forms a fixed connection of silicon particles and impurities removal during pressurization and ultrasonic washing, thereby achieving a microporous structure. ;

[0016] It can be seen from the above description that the present invention has the following advantages:

[0017] 1. The present invention solves the defects of existing diamond deposition. It utilizes the compressed deposition system of monosilane and methane to form gap filling on the diamond surface, effectively improving the problem of diamond roughness. At the same time, it cooperates with low-concentration deposition and active attraction of silicon element to ensure the doping and encapsulation characteristics of silicon element.

[0018] 2. The present invention utilizes a secondary deposition method to form diamond nucleation in-situ deposition, and cooperates with the mixed deposition of a silicon-carbon system to effectively achieve the nano-sizing and penetration of diamond particles, thereby improving the hardness and toughness of the fine steel stone particles.

[0019] 3. The present invention forms a homogenized concave-convex structure by means of surface treatment, limits carbon deposition based on the morphology of the deposition area, achieves semi-directional deposition, and serves the purpose of controlling methane deposition. DETAILED DESCRIPTION

[0020] The present invention is described in detail with reference to the embodiments, but no limitation is imposed on the claims of the present invention.

[0021] Example 1

[0022] A method for preparing silicon-doped nanodiamond grains comprises the following steps:

[0023] Step 1, grinding the silicon substrate;

[0024] Step 2, depositing diamond on the ground silicon substrate;

[0025] Step 3, performing secondary compression deposition on the deposited diamond;

[0026] Step 4, repeating steps 2 and 3, and ending with step 2, to obtain a silicon-doped diamond film;

[0027] Step 5: stripping the diamond film to obtain silicon-doped nano-diamond grains.

[0028] The grinding process in step 1 includes the following steps: a1, grinding the silicon substrate with diamond powder to roughen the surface of the silicon substrate, wherein the diamond powder is diamond powder of different particle sizes, and the diamond powder includes a first diamond powder with a particle size of 50nm and a second diamond powder with a particle size of 800nm, and the mass ratio of the first diamond powder to the second diamond powder is 2:2; the grinding pressure is 0.7MPa; a2, grinding the roughened silicon substrate with silicon particles to obtain a ground silicon substrate, wherein the silicon particles are silicon particles with a particle size of 500nm, and the grinding pressure is 2MPa a3, ultrasonically clean the ground silicon substrate, filter and dry it to obtain a clean silicon substrate, wherein the silicon substrate is ultrasonically treated with distilled water, ethanol and acetone in turn; the ultrasonic frequency of the distilled water is 60kHz, the temperature is 50°C, and the silicon substrate is taken out and dried after the ultrasonic treatment of the distilled water is completed, and the drying temperature is 110°C; the ultrasonic frequency of the ethanol is 50kHz, the temperature is 40°C, and the silicon substrate is removed and dried after the ultrasonic treatment of the ethanol is completed, and the drying temperature is 80°C; the ultrasonic frequency of the acetone is 40kHz, the temperature is 10°C, and the silicon substrate is removed and dried after the ultrasonic treatment of the acetone is completed, and the drying temperature is The temperature is 30°C; wherein the silicon particles adopt a microporous silicon particle structure, and the preparation method of the microporous silicon particle structure comprises the following steps: b1, adding sodium chloride to ethanol, and adding ethyl cellulose and stirring evenly to form a slurry, spray drying to obtain composite particles, wherein the mass ratio of sodium chloride to ethyl cellulose is 3:3, and the concentration of sodium chloride in ethanol is 300g / L, the spray drying rate is 5mL / min, and the temperature is 90°C; b2, putting nano silicon particles into distilled water and stirring evenly, then adding the composite particles and stirring well to form a suspension, and then drying and grinding after wet grinding and filtering. Grind to obtain prefabricated particles; the mass ratio of nano silicon particles to composite particles is 10:2, the mass ratio of the nano silicon particles to distilled water is 10:1, the grinding temperature is 5-10°C, the pressure is 2MPa, the dry grinding temperature is 20°C, and the grinding pressure is 4MPa; b3, pressurize the prefabricated particles for 2h, then soak them in an ethanol aqueous solution for ultrasonic treatment for 20min, filter and dry to obtain microporous silicon particles, the pressure of the pressurization treatment is 20MPa, the temperature is room temperature, the volume proportion of ethanol in the ethanol aqueous solution is 50%, the ultrasonic frequency is 50kHz, and the temperature is 40°C;

[0029] The deposition in step 2 adopts a chemical vapor deposition method, wherein the chemical vapor deposition uses methane as a carbon source, and is combined with hydrogen and nitrogen to form a reaction gas, the gas pressure is 10kPa, the microwave power is 600W, the substrate temperature during deposition is 800°C, and the deposition time is 10h. Furthermore, in the reaction gas in the deposition, the volume proportion of methane is 5%, the volume proportion of hydrogen is 10%, and the balance is nitrogen;

[0030] The compression deposition in step 3 adopts microwave vapor deposition, the reaction gas of the microwave vapor deposition is a silicon-containing reaction gas, and the silicon-containing reaction gas is a mixed gas of monosilane, methane, hydrogen and nitrogen, and the volume proportion of monosilane is 0.2%, the volume proportion of methane is 3%, the volume proportion of hydrogen is 13%, and the balance is nitrogen. The microwave power is 800W, the pressure is 20kPa, and the pressure is gradually compressed to 60kPa before deposition. The temperature during deposition rises to 800°C within 0.5h; the deposition time is 3h;

[0031] The stripping treatment in step 5 is carried out by acid corrosion, wherein the acid is a mixture of hydrofluoric acid and nitric acid, and the mass ratio of the hydrofluoric acid to the nitric acid is 2:1.

[0032] According to the test, the number ratio of the diamond grains in the range of 200-300 nm is 90%, and the silicon doping amount is 8300 ppm.

[0033] Example 2

[0034] A method for preparing silicon-doped nanodiamond grains comprises the following steps:

[0035] Step 1, grinding the silicon substrate;

[0036] Step 2, depositing diamond on the ground silicon substrate;

[0037] Step 3, performing secondary compression deposition on the deposited diamond;

[0038] Step 4, repeating steps 2 and 3, and ending with step 2, to obtain a silicon-doped diamond film;

[0039] Step 5: stripping the diamond film to obtain silicon-doped nano-diamond grains.

[0040] The grinding process in step 1 includes the following steps: a1, grinding the silicon substrate with diamond powder to roughen the surface of the silicon substrate, wherein the diamond powder is diamond powder of different particle sizes, and the diamond powder includes a first diamond powder with a particle size of 80nm and a second diamond powder with a particle size of 1300nm, and the mass ratio of the first diamond powder to the second diamond powder is 2:5; the grinding pressure is 0.9MPa; a2, grinding the roughened silicon substrate with silicon particles to obtain a ground silicon substrate, wherein the silicon particles are silicon particles with a particle size of 1000nm, and the grinding pressure is 4MPa. a; a3, ultrasonically cleaning the ground silicon substrate, filtering and drying to obtain a clean silicon substrate, wherein the silicon substrate is ultrasonically treated with distilled water, ethanol and acetone in sequence; the ultrasonic frequency of the distilled water is 80kHz, the temperature is 60°C, and the silicon substrate is taken out and dried after the ultrasonic treatment of the distilled water is completed, and the drying temperature is 120°C; the ultrasonic frequency of the ethanol is 60kHz, the temperature is 50°C, and the silicon substrate is removed and dried after the ultrasonic treatment of the ethanol is completed, and the drying temperature is 90°C; the ultrasonic frequency of the acetone is 50kHz, the temperature is 20°C, and the silicon substrate is removed and dried after the ultrasonic treatment of the acetone is completed, and the drying temperature is The temperature is 40°C; wherein the silicon particles adopt a microporous silicon particle structure, and the preparation method of the microporous silicon particle structure comprises the following steps: b1, adding sodium chloride to ethanol, and adding ethyl cellulose and stirring evenly to form a slurry, spray drying to obtain composite particles, the mass ratio of sodium chloride to ethyl cellulose is 3:4, and the concentration of sodium chloride in ethanol is 500g / L, the spray drying spray speed is 10mL / min, and the temperature is 100°C; b2, putting nano silicon particles into distilled water and stirring evenly, then adding the composite particles and stirring fully to form a suspension, and after wet grinding and filtering Dry grinding to obtain prefabricated particles; the mass ratio of nano silicon particles to composite particles is 10:3, the mass ratio of the nano silicon particles to distilled water is 10:2, the grinding temperature is 10°C, the pressure is 4MPa, the dry grinding temperature is 30°C, and the grinding pressure is 8MPa; b3, pressurizing the prefabricated particles for 3h, then immersing them in an ethanol aqueous solution for ultrasonic treatment for 30min, filtering and drying to obtain microporous silicon particles, the pressurizing pressure is 40MPa, the temperature is room temperature, the volume proportion of ethanol in the ethanol aqueous solution is 60%, the ultrasonic frequency is 70kHz, and the temperature is 60°C;

[0041] The deposition in step 2 adopts a chemical vapor deposition method, wherein the chemical vapor deposition uses methane as a carbon source, and is combined with hydrogen and nitrogen to form a reaction gas, the gas pressure is 15kPa, the microwave power is -800W, the substrate temperature during deposition is 1000°C, and the deposition time is 20h. Furthermore, in the reaction gas in the deposition, the volume proportion of methane is 8%, the volume proportion of hydrogen is 14%, and the balance is nitrogen;

[0042] The compression deposition in step 3 adopts microwave vapor deposition, the reaction gas of the microwave vapor deposition is a silicon-containing reaction gas, and the silicon-containing reaction gas is a mixed gas of monosilane, methane, hydrogen and nitrogen, and the volume proportion of monosilane is 0.5%, the volume proportion of methane is 7%, the volume proportion of hydrogen is 15%, and the balance is nitrogen. The microwave power is 1000W, the pressure is 50kPa, and the pressure is gradually compressed to 80kPa before deposition. The temperature during deposition rises to 900°C within 0.5h; the deposition time is 6h;

[0043] The stripping treatment in step 5 is carried out by acid corrosion, wherein the acid is a mixture of hydrofluoric acid and nitric acid, and the mass ratio of the hydrofluoric acid to the nitric acid is 2:1.

[0044] According to the test, the proportion of diamond grains in the range of 150-250 nm is 93%, and the silicon doping amount is 9150 ppm.

[0045] Example 3

[0046] A method for preparing silicon-doped nanodiamond grains comprises the following steps:

[0047] Step 1, grinding the silicon substrate;

[0048] Step 2, depositing diamond on the ground silicon substrate;

[0049] Step 3, performing secondary compression deposition on the deposited diamond;

[0050] Step 4, repeating steps 2 and 3, and ending with step 2, to obtain a silicon-doped diamond film;

[0051] Step 5: stripping the diamond film to obtain silicon-doped nano-diamond grains.

[0052] The grinding process in step 1 includes the following steps: a1, grinding the silicon substrate with diamond powder to roughen the surface of the silicon substrate, wherein the diamond powder is diamond powder of different particle sizes, and the diamond powder includes a first diamond powder with a particle size of 70nm and a second diamond powder with a particle size of 1000nm, and the mass ratio of the first diamond powder to the second diamond powder is 2:3; the grinding pressure is 0.8MPa; a2, grinding the roughened silicon substrate with silicon particles to obtain a ground silicon substrate, wherein the silicon particles are silicon particles with a particle size of 600nm, and the grinding pressure is 3MPa. a; a3, ultrasonically clean the ground silicon substrate, filter and dry it to obtain a clean silicon substrate, wherein the silicon substrate is ultrasonically treated with distilled water, ethanol and acetone in sequence; the ultrasonic frequency of the distilled water is 70kHz, the temperature is 55°C, and the silicon substrate is taken out and dried after the ultrasonic treatment of the distilled water is completed, and the drying temperature is 115°C; the ultrasonic frequency of the ethanol is 55kHz, the temperature is 45°C, and the silicon substrate is removed and dried after the ultrasonic treatment of the ethanol is completed, and the drying temperature is 85°C; the ultrasonic frequency of the acetone is 45kHz, the temperature is 15°C, and the silicon substrate is removed and dried after the ultrasonic treatment of the acetone is completed, and the drying The temperature is 35°C; wherein the silicon particles adopt a microporous silicon particle structure, and the preparation method of the microporous silicon particle structure comprises the following steps: b1, adding sodium chloride to ethanol, and adding ethyl cellulose and stirring evenly to form a slurry, spray drying to obtain composite particles, the mass ratio of sodium chloride to ethyl cellulose is 3:4, and the concentration of sodium chloride in ethanol is 400g / L, the spray drying spray speed is 8mL / min, and the temperature is 95°C; b2, putting nano silicon particles into distilled water and stirring evenly, then adding the composite particles and stirring fully to form a suspension, and after wet grinding and filtering The prefabricated particles are obtained by dry grinding; the mass ratio of nano silicon particles to composite particles is 10:3, the mass ratio of the nano silicon particles to distilled water is 10:1, the grinding temperature is 8°C, the pressure is 3MPa, the dry grinding temperature is 25°C, and the grinding pressure is 6MPa; b3, the prefabricated particles are pressurized for 3h, then immersed in an ethanol aqueous solution for ultrasonic treatment for 25min, filtered and dried to obtain microporous silicon particles, the pressure of the pressurized treatment is 30MPa, the temperature is room temperature, the volume proportion of ethanol in the ethanol aqueous solution is 55%, the ultrasonic frequency is 60kHz, and the temperature is 50°C;

[0053] The deposition in step 2 adopts a chemical vapor deposition method, wherein the chemical vapor deposition uses methane as a carbon source, and is combined with hydrogen and nitrogen to form a reaction gas, the gas pressure is 12 kPa, the microwave power is 700 W, the substrate temperature during deposition is 900 ° C, and the deposition time is 15 hours. Furthermore, in the reaction gas in the deposition, the volume proportion of methane is 7%, the volume proportion of hydrogen is 12%, and the balance is nitrogen;

[0054] The compression deposition in step 3 adopts microwave vapor deposition, the reaction gas of the microwave vapor deposition is a silicon-containing reaction gas, and the silicon-containing reaction gas is a mixed gas of monosilane, methane, hydrogen and nitrogen, and the volume proportion of monosilane is 0.4%, the volume proportion of methane is 4%, the volume proportion of hydrogen is 14%, and the balance is nitrogen. The microwave power is 900W, the pressure is 40kPa, and the pressure is gradually compressed to 70kPa before deposition. The temperature during deposition rises to 850°C within 0.5h; the deposition time is 5h;

[0055] The stripping treatment in step 5 is carried out by acid corrosion, wherein the acid is a mixture of hydrofluoric acid and nitric acid, and the mass ratio of the hydrofluoric acid to the nitric acid is 2:1.

[0056] According to the test, the proportion of diamond grains in the range of 200-300 nm is 92%, and the silicon doping amount is 8700 ppm.

[0057] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A method for preparing silicon-doped nanodiamond grains, characterized in that: The steps include: Step 1, grinding the silicon substrate; Step 2, depositing diamond on the ground silicon substrate; Step 3, performing secondary compression deposition on the deposited diamond; Step 4, repeating steps 2 and 3 to obtain a silicon-doped diamond film; Step 5, exfoliating the diamond film to obtain silicon-doped nano-diamond grains; the grinding process in step 1 includes the following steps: a1, grinding the silicon substrate with diamond powder to roughen the surface of the silicon substrate, the diamond powder uses diamond powder of different particle sizes, and the diamond powder includes a first diamond powder with a particle size of 50-80nm and a second diamond powder with a particle size of 800-1300nm, and the mass ratio of the first diamond powder to the second diamond powder is 2:2-5; the grinding pressure is 0.7-0.9MPa; a2 , grinding a roughened silicon substrate with silicon particles to obtain a ground silicon substrate, wherein the silicon particles have a particle size of 500-1000nm and a grinding pressure of 2-4MPa; a3, ultrasonically cleaning the ground silicon substrate, filtering and drying to obtain a clean silicon substrate, wherein the silicon substrate is ultrasonically treated with distilled water, ethanol and acetone in sequence, wherein the silicon particles in a2 have a microporous silicon particle structure, and the preparation method of the microporous silicon particle structure comprises the following steps: b1, adding sodium chloride to ethanol, and adding ethyl cellulose Stir evenly to form a slurry, and spray dry to obtain composite particles, wherein the mass ratio of sodium chloride to ethyl cellulose is 3:3-4, and the concentration of sodium chloride in ethanol is 300-500g / L, the spray drying rate is 5-10mL / min, and the temperature is 90-100°C; b2, put the nano silicon particles into distilled water and stir evenly, then add the composite particles and stir well to form a suspension, wet grind and filter, and then dry and grind to obtain prefabricated particles; the mass ratio of the nano silicon particles to the composite particles is 10:2-3, the nano silicon particles and distilled water The mass is 10:1-2, the grinding temperature is 5-10℃, the pressure is 2-4MPa, the dry grinding temperature is 20-30℃, and the grinding pressure is 4-8MPa; b3, the prefabricated particles are pressurized for 2-3h, then immersed in an ethanol aqueous solution for ultrasonic treatment for 20-30min, and filtered and dried to obtain microporous silicon particles, the pressure of the pressurized treatment is 20-40MPa, the temperature is room temperature, the volume proportion of ethanol in the ethanol aqueous solution is 50-60%, the ultrasonic frequency is 50-70kHz, and the temperature is 40-60℃.

2. The method for preparing silicon-doped nanodiamond grains according to claim 1, characterized in that: The deposition in step 2 adopts a chemical vapor deposition method, wherein methane is used as a carbon source, and hydrogen and nitrogen are combined to form a reaction gas, the gas pressure is 10-15 kPa, and the microwave power is 600-800W.

3. The method for preparing silicon-doped nano-diamond grains according to claim 2, characterized in that: The substrate temperature during deposition is 800-1000°C and the deposition time is 10-20h.

4. The method for preparing silicon-doped nano-diamond grains according to claim 2, characterized in that: In the reaction gas during the deposition, methane accounts for 5-8% by volume, hydrogen accounts for 10-14% by volume, and the remainder is nitrogen.

5. The method for preparing silicon-doped nano-diamond grains according to claim 1, characterized in that: The compressed deposition in step 3 adopts microwave vapor deposition, and the reaction gas of the microwave vapor deposition is a silicon-containing reaction gas, and the silicon-containing reaction gas is a mixed gas of monosilane, methane, hydrogen and nitrogen, the volume proportion of monosilane is 0.2-0.5%, the volume proportion of methane is 3-7%, the volume proportion of hydrogen is 13-15%, and the balance is nitrogen. The microwave power is 800-1000W.

6. The method for preparing silicon-doped nano-diamond grains according to claim 5, characterized in that: The pressure is 20-50 kPa, and the pressure is gradually compressed to 60-80 kPa before deposition.

7. The method for preparing silicon-doped nano-diamond grains according to claim 5, characterized in that: The temperature during deposition rises to 800-900°C within 0.5h; the deposition time is 3-6h.

8. The method for preparing silicon-doped nano-diamond grains according to claim 1, characterized in that: The stripping treatment in step 5 is carried out by acid corrosion, wherein the acid is a mixture of hydrofluoric acid and nitric acid, and the mass ratio of the hydrofluoric acid to the nitric acid is 2:1.

Citation Information

Patent Citations

  • Growth method of high-compactness nano diamond film

    CN102212795A

  • Method for preparing silicon-doped micro-nano composite diamond film through chemical vapor deposition (CVD)

    CN103757600A

  • Method for preparing tungsten carbide transition layer-silicon-doped diamond composite coating on steel substrates

    CN110735126A

  • Preparation method of high-brightness silicon vacancy color centers in nano-diamond

    CN111099586A

  • Self-supporting ultra-fine nanocrystalline diamond thick film

    US20210140038A1