A method for anti-oxidation argon arc welding of a titanium alloy actuator with a threaded small nozzle
By using a high-purity argon gas protection device during the argon arc welding process, the oxidation problem of the small threaded nozzle of the TA15 titanium alloy actuator cylinder of the aero-engine was solved, realizing efficient oxidation-free argon arc welding, avoiding the loss of high-value titanium alloy and improving welding quality.
Patent Information
- Application Number
- CN202211355278.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-01
AI Technical Summary
The narrow space of the threaded small nozzle on the TA15 titanium alloy actuator cylinder of the aircraft engine makes it difficult to perform argon arc welding and inconvenient to protect the welding torch, resulting in severe oxidation of the weld and heat-affected zone. In addition, titanium alloy is expensive, resulting in significant losses.
The process employs an anti-oxidation argon arc welding technique using a titanium alloy actuator cylinder with a threaded small nozzle. High-purity argon gas is introduced into an independent semi-enclosed cavity for protection, ensuring that the weld seam and heat-affected zone at the threaded small nozzle do not oxidize during the welding process. The two weld seams of the part are welded alternately in two stages, and are always cooled under argon gas protection.
It effectively prevented oxidation, avoided significant losses, recovered over 1 million yuan in economic losses, and improved welding efficiency and quality.
Smart Images

Figure CN115673486B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of argon arc welding devices for titanium alloy actuators in aviation engines, and in particular to an anti-oxidation argon arc welding process method for a titanium alloy actuator with a threaded small nozzle. Background Art
[0002] The threaded small nozzle on the TA15 titanium alloy actuator of the aircraft engine has a narrow space, which makes argon arc welding difficult and inconvenient to protect the welding gun. The weld and heat-affected zone at the threaded small nozzle are severely oxidized, resulting in scrapping. The titanium alloy actuator is expensive and the loss is large. In addition, the titanium alloy cylinder is thick, the heat input is large, the titanium alloy is difficult to dissipate heat, and the high temperature stays for a long time, which worsens the oxidation. Summary of the invention
[0003] In order to solve the above technical problems, an argon gas shielded welding device and welding process for a titanium alloy actuator with a threaded small nozzle are proposed. The specific technical solution is as follows:
[0004] A method for anti-oxidation argon arc welding of a titanium alloy actuator with a threaded small nozzle comprises the following steps:
[0005] Step 1: Preparation before welding
[0006] The titanium alloy cylinder to be welded is polished with an abrasive belt to remove the film; the threaded small nozzle with a thickness of 2mm and a groove of 1mm×1mm to be welded is polished with an abrasive belt; the titanium alloy cylinder, the threaded small nozzle and the titanium alloy welding wire are pickled and hydrogen-fixed together, and then dried and packed into a plastic film, and then vacuumized for packaging and turnover;
[0007] Step 2: Weld the threaded small nozzle A on one side
[0008] The interval between pickling and welding of the titanium alloy cylinder shall not exceed 120 hours. Open the package and put the titanium alloy cylinder into the cylinder groove of the base. Turn the threaded small nozzle A to the matching compartment A, cover the cover plate A, place the threaded small nozzle A as a whole in the compartment A, and only expose the part to be welded. Fill the ventilation pipe A with high-purity argon gas. The argon gas fills the compartment A from the four rows of small holes. After filling for 2 minutes, perform argon arc welding to complete the welding of this side. After the welding is completed, the welding gun continues to stay for ventilation for more than 2 minutes;
[0009] Step 3: Weld the threaded small nozzle B on one side
[0010] Transfer the threaded small connector B to the compartment B, cover it with cover plate B, fill the vent pipe B with high-purity argon gas, and perform the rest of the same operations as the threaded small connector A to complete the welding of one side of the threaded small connector B. At this time, the threaded small connector A has been completely cooled;
[0011] Step 4: Weld the other side of the threaded small nozzle A
[0012] Open the cover plates A and B, transfer the threaded small nozzle A to the matching compartment C, cover the cover plate C, place the threaded small nozzle A as a whole in the compartment C, and only expose the part to be welded. Fill the ventilation pipe C with high-purity argon gas. The argon gas fills the compartment C from the four rows of small holes. After filling for 2 minutes, perform argon arc welding to complete the welding of the other side of the threaded small nozzle A. After the welding is completed, the welding gun continues to stay for ventilation for more than 2 minutes;
[0013] Step 5: Weld the other side of the threaded small nozzle B
[0014] Transfer the threaded small nozzle B to the compartment D, cover it with the cover plate D, fill the vent pipe D with high-purity argon gas, and perform the rest of the same operations as the threaded small nozzle A to complete the welding of the other side of the threaded small nozzle B; after the welding is completed, the welding gun continues to ventilate for more than 2 minutes, and the threaded small nozzle B is cooled down. At this time, the threaded small nozzle A has been completely cooled down;
[0015] At this time, the titanium alloy cylinder is completely welded, and the threaded small nozzle A and the threaded small nozzle B are welded without oxidation argon arc; remove the titanium alloy cylinder, and continue to weld the next piece in the same way.
[0016] The protective welding device using the process method includes a substrate, a cover plate A, a cover plate B, a cover plate C, a cover plate D, a vent pipe A, a vent pipe B, a vent pipe C and a vent pipe D;
[0017] The base body is a U-shaped rectangular parallelepiped, with a cylinder groove matching the titanium alloy cylinder in the middle;
[0018] The base and the side wall of the barrel groove are symmetrically provided with compartments A, B, C and D extending from the upper end surface of the base to the inner cavity of the barrel groove;
[0019] The compartment A, compartment B, compartment C and compartment D are all independent semi-enclosed compartments;
[0020] The outer wall of the base on one side of the compartment C and the compartment D is provided with a cover plate C and a cover plate D;
[0021] The outer wall of the base on one side of the compartment A and the compartment B is provided with a cover plate A and a cover plate B;
[0022] The cover plates A, B, C and D can all be folded 180° to the upper end of the base body to seal the threaded small nozzle in the compartment for protection.
[0023] The vent pipe C and the vent pipe D symmetrically penetrate from one end of the base body and extend into the compartment C and the compartment D, and the vent pipe C and the vent pipe D are on the same axis;
[0024] The vent pipe A and the vent pipe B symmetrically penetrate from one end of the base body and extend into the compartment A and the compartment B, and the vent pipe A and the vent pipe B are on the same axis;
[0025] Small holes are arranged on the sections of the vent pipe A, vent pipe B8, vent pipe C and vent pipe D in the compartment A, compartment B, compartment C and compartment D.
[0026] The above-mentioned method for anti-oxidation argon arc welding of a titanium alloy actuator with a threaded small nozzle has a preferred embodiment in which, in step 2 and step 4, the argon gas flow rate is 6 L / min-8 L / min.
[0027] The described method for anti-oxidation argon arc welding of a titanium alloy actuator with a threaded small nozzle has a preferred embodiment in which the small hole in step 2 and step 4 is a small hole of φ1 mm.
[0028] The described method for anti-oxidation argon arc welding of a titanium alloy actuator with a threaded small nozzle has a preferred embodiment that, in step one, the titanium alloy welding wire is TA15 or TA1.
[0029] The present invention places the threaded small nozzle as a whole in an independent semi-enclosed compartment of the device, exposing only the part to be welded. The compartment is filled with high-purity argon gas during the entire welding and post-weld cooling process, so that the weld and heat-affected zone of the threaded small nozzle are not oxidized.
[0030] Each of the two welds of the part is welded twice, alternately, so that the weld is always protected by argon gas during welding and cooling. The device can effectively conduct heat and shorten the cooling time.
[0031] The present invention can effectively solve the problem of argon arc welding oxidation of the titanium alloy actuator cylinder with a threaded small nozzle of the TA15 aircraft engine, recover a large amount of losses, and avoid losses of more than 1 million yuan. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the front view of the TA15 titanium alloy actuator part with a small threaded nozzle;
[0033] Figure 2 This is the side view of the titanium alloy actuator part of TA15 with a small threaded nozzle;
[0034] Figure 3 This is a top view of the titanium alloy actuator part of TA15 with a small threaded nozzle;
[0035] Figure 4 This is the axonometric drawing of the titanium alloy actuator part of TA15 with a small threaded nozzle;
[0036] Figure 5 It is a top view of an argon gas shielded argon arc welding device;
[0037] Figure 6 This is a schematic diagram of the structure of an argon gas shielded argon arc welding device;
[0038] Figure 7It is a side view of an argon gas shielded argon arc welding device;
[0039] Figure 8 This is the front view of the argon gas shielded argon arc welding device;
[0040] Fig. 9 Schematic diagram of the installation of a TA15 titanium alloy actuator with a small threaded nozzle and an argon-shielded argon arc welding device a;
[0041] Fig.10 Installation diagram b of the TA15 titanium alloy actuator with a small threaded nozzle and the argon shielded argon arc welding device.
[0042] In the figure: 1-titanium alloy cylinder, 2-base, 3-cover plate A, 4-cover plate B, 5-cover plate C, 6-cover plate D, 7-ventilation pipe A, 8-ventilation pipe B, 9-ventilation pipe C, 10-ventilation pipe D, 11-cylinder groove, 12-threaded small nozzle A, 13-compartment A, 14-compartment B, 15-compartment C, 16-compartment D, 17-threaded small nozzle B, 18-small hole. DETAILED DESCRIPTION
[0043] The following is combined with Figure 1-10 The present invention is further described in detail with reference to the accompanying drawings and examples.
[0044] A method for anti-oxidation argon arc welding of a titanium alloy actuator with a threaded small nozzle comprises the following steps:
[0045] Step 1: Preparation before welding
[0046] The TA15 titanium alloy cylinder to be welded is polished with an abrasive belt to remove the film; the threaded small nozzle with a thickness of 2mm and a groove of 1mm×1mm to be welded is polished with an abrasive belt; the titanium alloy cylinder, the threaded small nozzle and the titanium alloy welding wire TA1 are pickled and hydrogen-fixed together, and then dried and packed into a plastic film, and then vacuumized for packaging and turnover;
[0047] Step 2: Weld the threaded small nozzle A12 on one side
[0048] The interval between the pickling and the completion of welding of the titanium alloy cylinder 1 shall not exceed 120 hours. Unpack and place the titanium alloy cylinder 1 into the cylinder groove 11 of the base 2. Turn the threaded small nozzle A12 into the matching compartment A. Cover the cover A. Place the threaded small nozzle A12 in the compartment A13 as a whole, leaving only the part to be welded exposed. Fill the ventilation pipe A7 with high-purity argon gas. The argon gas fills the compartment A13 from four rows of φ1mm small holes 18. The argon gas flow rate is 6 L / min-8L / min. After filling for 2 minutes, perform argon arc welding to complete the welding of this side. After the welding is completed, the welding gun continues to stay for ventilation for more than 2 minutes.
[0049] Step 3: Weld the threaded small nozzle B17 on one side
[0050] Transfer the threaded small connector B17 to the compartment B14, cover it with the cover plate B4, fill the vent pipe B8 with high-purity argon gas, and perform the rest of the same operations as the threaded small connector A to complete the welding of one side of the threaded small connector B17. At this time, the threaded small connector A has been completely cooled;
[0051] Step 4: Weld the other side of the threaded small nozzle A
[0052] Open the cover plates A3 and B4, transfer the threaded small nozzle A12 to the matching compartment C15, cover the cover plate C5, place the threaded small nozzle A12 in the compartment C15 as a whole, and only expose the part to be welded. Fill the ventilation pipe C9 with high-purity argon gas. The argon gas fills the compartment C15 from the four rows of φ1mm small holes 18. The argon gas flow rate is 6 L / min-8L / min. After filling for 2 minutes, perform argon arc welding to complete the welding of the other side of the threaded small nozzle A12. After the welding is completed, the welding gun continues to stay for ventilation for more than 2 minutes;
[0053] Step 5: Weld the other side of the threaded small nozzle B17
[0054] Transfer the threaded small nozzle B17 to the compartment D16, cover it with the cover plate D6, fill the ventilation pipe D10 with high-purity argon gas, and perform the rest of the operations with the threaded small nozzle A12 to complete the welding of the other side of the threaded small nozzle B; after the welding is completed, the welding gun continues to ventilate for more than 2 minutes until the threaded small nozzle B17 cools down, at which time the threaded small nozzle A12 has completely cooled down;
[0055] At this time, all welding of the titanium alloy cylinder 1 is completed, and the threaded small nozzle A12 and the threaded small nozzle B17 are welded without oxidation; remove the titanium alloy cylinder 1, and continue to weld the next piece in the same way.
[0056] The welding device using the process method includes a base 2, a cover plate A3, a cover plate B4, a cover plate C5, a cover plate D6, a vent pipe A7, a vent pipe B8, a vent pipe C9 and a vent pipe D10;
[0057] The base body 2 is a U-shaped rectangular parallelepiped, and a cylinder groove 11 matching the titanium alloy cylinder body 1 is provided in the middle;
[0058] The base body 2 and the side wall of the barrel groove 11 are symmetrically provided with compartments A13, B14, C15 and D16 extending from the upper end surface of the base body 2 to the inner cavity of the barrel groove 11;
[0059] The compartment A13, compartment B14, compartment C15 and compartment D16 are all independent semi-enclosed compartments;
[0060] The outer wall of the base on one side of the compartment C15 and the compartment D16 is provided with a cover plate C5 and a cover plate D6;
[0061] The outer wall of the base on one side of the compartment A13 and the compartment B14 is provided with a cover plate A3 and a cover plate B4;
[0062] The cover plate A3, cover plate B4, cover plate C5, and cover plate D6 can all be folded 180° to the upper end of the base 2 to seal the threaded small nozzle in the compartment for protection;
[0063] The ventilation pipe C9 and the ventilation pipe D10 symmetrically penetrate from one end of the base body 2 and extend into the compartment C15 and the compartment D16, and the ventilation pipe C9 and the ventilation pipe D10 are on the same axis;
[0064] The ventilation pipe A7 and the ventilation pipe B8 symmetrically penetrate from one end of the base body 2 and extend into the compartment A13 and the compartment B14, and the ventilation pipe A7 and the ventilation pipe B8 are on the same axis;
[0065] Small holes 18 are provided on the sections of the ventilation pipes A7, B8, C9 and D10 in the compartments A13, B14, C15 and D16.
Claims
1. A method for anti-oxidation argon arc welding of a titanium alloy actuator with a threaded small nozzle, characterized in that: The steps include: Step 1: Preparation before welding The titanium alloy cylinder to be welded is polished with an abrasive belt to remove the film; the threaded small nozzle with a thickness of 2mm and a groove of 1mm×1mm to be welded is polished with an abrasive belt; the titanium alloy cylinder, the threaded small nozzle and the titanium alloy welding wire are pickled and hydrogen-fixed together, and then dried and packed into a plastic film, and then vacuumized for packaging and turnover; Step 2: Weld the threaded small nozzle A on one side The interval between pickling and welding of the titanium alloy cylinder shall not exceed 120 hours. Open the package and put the titanium alloy cylinder into the cylinder groove of the base. Turn the threaded small nozzle A to the matching compartment A, cover the cover plate A, place the threaded small nozzle A as a whole in the compartment A, and only expose the part to be welded. Fill the ventilation pipe A with high-purity argon gas. The argon gas fills the compartment A from the four rows of small holes. After filling for 2 minutes, perform argon arc welding to complete the welding of this side. After the welding is completed, the welding gun continues to stay for ventilation for more than 2 minutes; Step 3: Weld the threaded small nozzle B on one side Transfer the threaded small connector B to the compartment B, cover it with cover plate B, fill the vent pipe B with high-purity argon gas, and perform the rest of the same operations as the threaded small connector A to complete the welding of one side of the threaded small connector B. At this time, the threaded small connector A has been completely cooled; Step 4: Weld the other side of the threaded small nozzle A Open the cover plates A and B, transfer the threaded small nozzle A to the matching compartment C, cover the cover plate C, place the threaded small nozzle A as a whole in the compartment C, and only expose the part to be welded. Fill the ventilation pipe C with high-purity argon gas. The argon gas fills the compartment C from the four rows of small holes. After filling for 2 minutes, perform argon arc welding to complete the welding of the other side of the threaded small nozzle A. After the welding is completed, the welding gun continues to stay for ventilation for more than 2 minutes; Step 5: Weld the other side of the threaded small nozzle B Transfer the threaded small nozzle B to the compartment D, cover it with the cover plate D, fill the vent pipe D with high-purity argon gas, and perform the rest of the same operations as the threaded small nozzle A to complete the welding of the other side of the threaded small nozzle B; after the welding is completed, the welding gun continues to ventilate for more than 2 minutes, and the threaded small nozzle B is cooled down. At this time, the threaded small nozzle A has been completely cooled down; At this time, the titanium alloy cylinder is completely welded, and the threaded small nozzle A and the threaded small nozzle B are welded without oxidation by argon arc welding; remove the titanium alloy cylinder, and continue to weld the next piece in the same way; The protective welding device using the process method includes a substrate, a cover plate A, a cover plate B, a cover plate C, a cover plate D, a vent pipe A, a vent pipe B, a vent pipe C and a vent pipe D; The base body is a U-shaped rectangular parallelepiped, with a cylinder groove matching the titanium alloy cylinder in the middle; The base and the side wall of the barrel groove are symmetrically provided with compartments A, B, C and D extending from the upper end surface of the base to the inner cavity of the barrel groove; The compartment A, compartment B, compartment C and compartment D are all independent semi-enclosed compartments; The outer wall of the base on one side of the compartment C and the compartment D is provided with a cover plate C and a cover plate D; The outer wall of the base on one side of the compartment A and the compartment B is provided with a cover plate A and a cover plate B; The cover A, cover B, cover C, cover D can be folded 180 ° to the upper end of the base, for the threaded small nozzle closed in the compartment for protection; The vent pipe C and the vent pipe D symmetrically penetrate from one end of the base body and extend into the compartment C and the compartment D, and the vent pipe C and the vent pipe D are on the same axis; The vent pipe A and the vent pipe B symmetrically penetrate from one end of the base body and extend into the compartment A and the compartment B, and the vent pipe A and the vent pipe B are on the same axis; Small holes are arranged on the sections of the vent pipe A, vent pipe B8, vent pipe C and vent pipe D in the compartment A, compartment B, compartment C and compartment D.
2. The method for anti-oxidation argon arc welding of a titanium alloy actuator with a threaded small nozzle according to claim 1 is characterized in that: In step 2 and step 4, the argon gas flow rate is 6 L / min-8 L / min.
3. The method for anti-oxidation argon arc welding of a titanium alloy actuator with a threaded small nozzle according to claim 1 is characterized in that: In the step 2 and step 4, the small hole is a hole of φ1 mm.
4. The oxidation-proof argon arc welding process of a titanium alloy actuator with a threaded small nozzle according to claim 1 is characterized in that: In step 1, the titanium alloy welding wire is TA15 or TA1.