A flexible fluorescent piezoelectric sensor and its preparation method

By adopting a composite membrane structure of PVDF-HFP and CQDs in a flexible piezoelectric sensor, combined with an ITO-PEN electrode treated with oxygen plasma, the multifunctionality and self-energy problems are solved, and high resolution and colorful fluorescence functions are achieved. fluorescent piezoelectric sensors, suitable for smart systems and wearable devices.

CN115683408BActive Publication Date: 2024-11-01ANHUI LEADER TECHNOLOGY INNOVATION DEVELOPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211431716.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-11-01
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

Existing flexible piezoelectric sensors have shortcomings in terms of versatility and high flexibility, especially the lack of self-energy and fluorescence functions, which limit their application in wearable devices and smart systems.

Method used

PVDF-HFP is used as a piezoelectric material, combined with the particle-induced effect of CQDs and the oxygen plasma-enhanced ITO-PEN electrode, and a composite of PVDF-HFP piezoelectric layer/CQDs fluorescent layer/PVDF-HFP piezoelectric layer is prepared through a specific process. The film realizes the preparation of fluorescent piezoelectric sensors and has the dual functions of piezoelectric and fluorescence.

Benefits of technology

It realizes high resolution, high flexibility and self-energy fluorescent piezoelectric sensors, with colorful fluorescence functions of ultraviolet excitation, is suitable for large-scale production, and has wide application value in wearable devices and intelligent systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115683408B_ABST
    Figure CN115683408B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of sensor technology, and in particular, relates to a flexible fluorescent piezoelectric sensor and a preparation method thereof. The method includes PVDF-HFP solution configuration, CQDs suspension configuration, functional composite film preparation and sensor assembly. The flexible fluorescent piezoelectric sensor of the present invention adopts a sandwich structure of ITO-PEN electrode / fluorescent piezoelectric functional composite layer / ITO-PEN electrode, wherein the fluorescent piezoelectric functional composite layer is a functional composite film of a laminated structure of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer, which couples the particle induced effect and fluorescence effect of CQDs and the substrate induced effect of the ITO-PEN electrode enhanced by oxygen plasma, and has both piezoelectric and fluorescent dual functions. The flexible fluorescent piezoelectric sensor of the present invention has a simple preparation process and low raw material cost; the multi-function of the device is realized by using the multi-function of the material, thereby eliminating the cumbersome integration process of the device and the complex auxiliary electronic system, and is suitable for large-scale production applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sensors, and in particular relates to a flexible fluorescent piezoelectric sensor and a preparation method thereof. Background Art

[0002] With the continuous advancement of intelligent systems such as wearable electronic devices, intelligent robots, human / machine interaction (iHMI) and human health measurement in daily life, higher requirements are placed on the performance characteristics of tactile sensors. Among them, the four major performance characteristics of tactile sensors, namely high resolution, high flexibility, self-power supply and multi-function, are important challenges plaguing this field.

[0003] As a newcomer in the family of tactile sensors, flexible piezoelectric sensors have the advantages of high natural frequency, high sensitivity, high signal-to-noise ratio, and good stability. Flexible piezoelectric sensors are based on the piezoelectric effect and have the characteristics of self-power supply, that is, they can convert mechanical energy in the living environment into electrical energy. They can not only maintain their own work, but also store and utilize excess electrical energy, overcoming the major obstacle of additional power supply for wearable devices. On the premise of giving flexible piezoelectric sensors high sensitivity, high flexibility, and self-power supply, giving sensors multifunctionality through the multifunctionality of materials is an urgent need for the application of intelligent systems in daily life. For example, the invention patent with application number 202011091567.6 disclosed by this research group involves a titanium dioxide / carbon dot composite film pressure sensor and its preparation method, which is to mix CQDs and TiO2 to form a composite film, and together with the upper and lower electrodes to form a resistive pressure sensor. The introduction of CQDs enables the sensor to have the potential of a new function of colorful fluorescence on the basis of sensing pressure. However, due to the limitations of the characteristics of the core material and the rigid electrode material, this type of sensor does not have the characteristics of self-power supply and high flexibility.

[0004] Polyvinylidene fluoride (PVDF) (including derivatives PVDF-TrFE and PVDF-HFP) is currently the best flexible piezoelectric material with the advantages of high flexibility, high electromechanical coupling, good biocompatibility, high optical transparency and wide response range. PVDF is a semi-crystalline polymer whose electroactivity is determined by the β piezoelectric phase of the TTTT conformation. In order to form the β piezoelectric phase in PVDF, particle induced polarization is an effective means. The main idea of ​​particle induced polarization is to embed nanoparticles into PVDF to promote the formation of β phase while the material is being formed, so that the material has a piezoelectric effect. Particles such as BaTiO3, carbon black, ZnO, graphene, and carbon nanotubes (CNTs) all show induced polarization effects. For example, Si Wenyan et al. (Preparation and pressure sensing of low-voltage near-field electrospinning ZnO / PVDF composite micron fiber arrays. Journal of Chemistry in Universities, 2017, 38 (6): 997-1001) used near-field electrospinning to embed ZnO particles into PVDF to obtain ZnO / PVDF composite micron fiber arrays, and demonstrated the piezoelectric effect of the composite material. Zhang Yike et al. (Preparation and piezoelectric properties of carbon nanotube / polyvinylidene fluoride nanofiber membranes. Journal of Textile Research, 2021, 42 (3): 44-50) used electrospinning to introduce CNTs into PVDF nanofiber membranes to prepare CNTs / PVDF nanofiber membranes, and assembled them into flexible piezoelectric sensors with sandwich structures. However, these studies did not solve the problem of the multifunctionality of the sensor, that is, they were limited to piezoelectric functions.

[0005] Carbon quantum dots (CQDs) have good photoluminescence, resistance to photobleaching, chemical stability and a wide range of raw materials. They have shown unique charm in the fields of fluorescent labeling, bioimaging and sensing, and light-emitting diodes. Dong Li et al. (Preparation of UV-shielding PVDF composite film using carbon quantum dots. Engineering Plastics Application, 2020, 48 (3): 125-129) provided a method for preparing UV-shielding PVDF film, attaching CQDs / polyvinyl alcohol (PVAL) composite film to the two surfaces of PVDF film to form a UV-shielding layer, highlighting the UV-shielding function of the material. When applying the above materials to sensors, there are still two huge challenges: first, CQDs do not play a role in inducing the formation of β phase in PVDF, that is, the composite material will have no piezoelectric effect or have a very weak piezoelectric effect; second, CQDs in PVAL cannot effectively avoid Förster energy transfer due to agglomeration, so that the composite film has no fluorescence effect. Summary of the invention

[0006] The present invention aims to meet the urgent demands for four major performance characteristics of high resolution, high flexibility, self-power supply and multi-function faced in the application of tactile sensors. In view of the shortcomings of the existing technology, PVDF with piezoelectric effect is used as the pressure-sensitive material, and the particle induced effect and fluorescence effect of CQDs and the substrate induced effect of ITO-PEN electrode enhanced by oxygen plasma are coupled. A flexible fluorescent piezoelectric sensor is prepared by a specific process. The sensor uses a composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer as a fluorescent piezoelectric functional composite material. On the basis of maintaining high resolution, high flexibility and self-power supply of the device, with the help of the fluorescence characteristics of highly dispersed CQDs, the device is given a new function of colorful fluorescence excited by ultraviolet light through the multifunctionalization of the material.

[0007] The specific technical solutions of the present invention are as follows:

[0008] A method for preparing a flexible fluorescent piezoelectric sensor comprises the following steps:

[0009] (1) Preparation of PVDF-HFP solution: N,N-dimethylformamide and additive were mixed and stirred at a mass ratio of 1: (0.2-1) for 10-30 min to obtain solution a; then PVDF-HFP and solution a were mixed and stirred at a mass ratio of 1: (5-10) for 2-4 h to obtain PVDF-HFP solution;

[0010] (2) Preparation of CQDs suspension: CQDs and water were mixed in a mass ratio of 1:(5-20) and ultrasonicated for 30-120 min to obtain a CQDs suspension;

[0011] (3) Preparation of functional composite film: The conductive surface of the ITO-PEN electrode is treated with oxygen plasma, and then the PVDF-HFP solution is coated on the conductive surface of the ITO-PEN electrode, and a PVDF-HFP piezoelectric layer is formed by heat treatment. Subsequently, a CQDs suspension is coated on the PVDF-HFP piezoelectric layer, and a CQDs fluorescent layer is formed by drying. Finally, the PVDF-HFP solution is coated on the CQDs fluorescent layer again, and a PVDF-HFP piezoelectric layer is formed by heat treatment, thereby obtaining an ITO-PEN electrode with a functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited on one side;

[0012] (4) Sensor assembly: Place the ITO-PEN electrode with the functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited above with one side facing up, and then take another blank ITO-PEN electrode with the conductive surface facing down, and cover its upper surface in an offset manner. The uncovered parts of the two electrodes are used as leads, and silicone is coated around them for fixation. The wires are fixed to the leads of the two electrodes by conductive silver paste, thus obtaining a flexible fluorescent piezoelectric sensor.

[0013] In step (1), the additive is one or more of acetone, ethanol, methyl ethyl ketone, and ethyl acetate.

[0014] In step (3), the oxygen plasma treatment time is 5 to 15 minutes.

[0015] In step (3), coating is carried out by any one of spin coating, scraper coating, screen printing and casting.

[0016] In step (3), the coating thicknesses of the PVDF-HFP piezoelectric layer and the CQDs fluorescent layer are 10~50µm and 10~50µm, respectively.

[0017] In step (3), the specific steps of heat treatment are: first standing at room temperature for 30 to 120 minutes, and then keeping warm at 100 to 120°C for 1 to 2 hours.

[0018] In step (3), the specific steps of drying are: keeping warm at 100-120°C for 1-2 hours.

[0019] In step (4), the overlapping portion of the two electrodes accounts for 70-80% of the surface area of ​​a single electrode.

[0020] In summary, the present invention has the following beneficial effects:

[0021] (1) The flexible fluorescent piezoelectric sensor of the present invention adopts a sandwich structure of ITO-PEN electrode / fluorescent piezoelectric functional composite layer / ITO-PEN electrode, wherein the fluorescent piezoelectric functional composite layer is a functional composite film of a laminated structure of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer, which couples the particle induced effect and fluorescence effect of CQDs and the substrate induced effect of the ITO-PEN electrode enhanced by oxygen plasma, and has both piezoelectric and fluorescent functions. The piezoelectric function comes from the β piezoelectric phase in PVDF, and its formation path is that the substrate induced effect of organic functional groups such as hydroxyl (-OH) on the surface of the ITO-PEN electrode after oxygen plasma treatment promotes the formation of the β piezoelectric phase in the PVDF-HFP piezoelectric layer thereon, and the particle induced effect of the CQDs fluorescent layer promotes the formation of the β piezoelectric phase in another PVDF-HFP piezoelectric layer thereon; the fluorescent function comes from the CQDs fluorescent layer, and these CQDs exist in a single quantum state and are highly dispersed, thereby effectively avoiding Foster energy transfer. At the same time, by using different fluorescent CQDs, the sensor can be given colorful fluorescence.

[0022] (2) The flexible fluorescent piezoelectric sensor of the present invention has a simple preparation process and low raw material cost. The multifunctionality of the device is achieved by leveraging the multifunctionality of the material, thereby eliminating the cumbersome integration process and complex auxiliary electronic system of the device, making it suitable for large-scale production applications.

[0023] (3) The flexible fluorescent piezoelectric sensor prepared by the present invention has great application value in intelligent systems such as wearable electronic devices, intelligent robots, human / machine interaction and human health measurement. For example, when used as the electronic skin of intelligent robots, it enhances tactile perception and also gives new functions such as light wave perception, fluorescent self-warning and fluorescent anti-counterfeiting; when used for dynamic monitoring of human health, in addition to obtaining information such as pulse, it also has a new fluorescent self-warning function that can sense ultraviolet rays in the environment through its own color changes; when used in wearable devices, the enhanced ultraviolet barrier will better protect the human body from ultraviolet damage. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the structure of the flexible fluorescent piezoelectric sensor in an embodiment of the present invention.

[0025] Figure 2 is the fluorescence spectrum of the flexible fluorescent piezoelectric sensor in the embodiment of the present invention.

[0026] Figure 3 This is a macroscopic photograph of the flexible fluorescent piezoelectric sensor in the embodiment of the present invention under the excited fluorescence state.

[0027] Figure 4It is a real-time output voltage-time curve of the flexible fluorescent piezoelectric sensor under periodic constant force in an embodiment of the present invention.

[0028] Figure 5 1 is a real-time output voltage-force curve of the flexible fluorescent piezoelectric sensor in an embodiment of the present invention. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described below with specific embodiments, but the specific details of the embodiments are only for illustrating the present invention and do not represent all technical methods under the concept of the present invention. Therefore, it should not be understood as limiting the overall technical solution of the present invention.

[0030] A method for preparing a flexible fluorescent piezoelectric sensor comprises the following steps:

[0031] (1) Preparation of PVDF-HFP solution: N,N-dimethylformamide and additive are mixed and stirred at a mass ratio of 1: (0.2-1) for 10-30 minutes to obtain solution a; PVDF-HFP and solution a are then mixed and stirred at a mass ratio of 1: (5-10) for 2-4 hours to obtain PVDF-HFP solution; the additive is one or more of acetone, ethanol, methyl ethyl ketone, and ethyl acetate;

[0032] (2) Preparation of CQDs suspension: CQDs and water were mixed in a mass ratio of 1:(5-20) and ultrasonicated for 30-120 min to obtain a CQDs suspension;

[0033] (3) Preparation of functional composite film: The conductive surface of the ITO-PEN electrode is treated with oxygen plasma, and then the PVDF-HFP solution is coated on the conductive surface of the ITO-PEN electrode, and a PVDF-HFP piezoelectric layer is formed by heat treatment. Subsequently, a CQDs suspension is coated on the PVDF-HFP piezoelectric layer, and a CQDs fluorescent layer is formed by drying. Finally, the PVDF-HFP solution is coated on the CQDs fluorescent layer again, and a PVDF-HFP piezoelectric layer is formed by heat treatment, thereby obtaining an ITO-PEN electrode with a functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited on one side;

[0034] The oxygen plasma treatment time is 5-15 minutes; the coating is carried out by any one of spin coating, scraper coating, screen printing and casting; the coating thickness of the PVDF-HFP piezoelectric layer and the CQDs fluorescent layer are 10-50µm and 10-50µm respectively; the specific steps of heat treatment are: first standing at room temperature for 30-120 minutes, and then keeping warm at 100-120°C for 1-2 hours; the specific steps of drying are: keeping warm at 100-120°C for 1-2 hours;

[0035] (4) Sensor assembly: Place the ITO-PEN electrode with the functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited above with one side facing up, and then take another blank ITO-PEN electrode with the conductive surface facing down and cover its upper surface in an offset manner. The uncovered parts of the two electrodes are used as leads, and silicone is coated around them for fixation. The wires are fixed to the leads of the two electrodes with conductive silver paste to obtain a flexible fluorescent piezoelectric sensor; the overlapping part of the two electrodes accounts for 70-80% of the surface area of ​​a single electrode.

[0036] The flexible fluorescent piezoelectric sensor of the present invention is composed of ITO-PEN electrodes, PVDF-HFP piezoelectric layers, CQDs fluorescent layers, PVDF-HFP piezoelectric layers and ITO-PEN electrodes stacked in sequence. The uncovered parts of the two electrodes are used as leads. The wires are fixed at the leads of the two electrodes by conductive silver paste. The schematic diagram of the structure is shown in FIG. Figure 1 .

[0037] The preparation method of the present invention is further described in detail below through specific examples.

[0038] Example 1

[0039] A method for preparing a flexible fluorescent piezoelectric sensor comprises the following steps:

[0040] (1) Preparation of PVDF-HFP solution: N,N-dimethylformamide and acetone were mixed and stirred at a mass ratio of 1:0.56 for 20 minutes to obtain solution a; then PVDF-HFP and solution a were mixed and stirred at a mass ratio of 1:7.37 for 2 hours to obtain PVDF-HFP solution;

[0041] (2) Preparation of CQDs suspension: CQDs and water were mixed at a mass ratio of 1:10 and ultrasonicated for 60 min to obtain a CQDs suspension;

[0042] (3) Preparation of functional composite film: The conductive surface of the ITO-PEN electrode was treated with oxygen plasma for 5 min, and then the PVDF-HFP solution was spin-coated on the conductive surface of the ITO-PEN electrode, and then the surface was kept at room temperature for 30 min and then kept at 120°C for 1 h to form a PVDF-HFP piezoelectric layer. Subsequently, the CQDs suspension was spin-coated on the PVDF-HFP piezoelectric layer and kept at 120°C for 1 h to form a CQDs fluorescent layer. Finally, the PVDF-HFP solution was spin-coated on the CQDs fluorescent layer again, and then the surface was kept at room temperature for 30 min and then kept at 120°C for 1 h to form a PVDF-HFP piezoelectric layer. An ITO-PEN electrode with a functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer was obtained. The coating thicknesses of the PVDF-HFP piezoelectric layer and the CQDs fluorescent layer were 30 µm and 30 µm, respectively.

[0043] (4) Sensor assembly: Place the ITO-PEN electrode with the functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited above with one side facing up, and then take another blank ITO-PEN electrode with the conductive surface facing down and cover its upper surface in an offset manner. The uncovered parts of the two electrodes are used as leads, which are fixed by coating silicone around them. The wires are fixed to the leads of the two electrodes by conductive silver paste, thus obtaining a flexible fluorescent piezoelectric sensor; wherein the overlapping part of the two electrodes accounts for 75% of the surface area of ​​a single electrode.

[0044] Example 2

[0045] A method for preparing a flexible fluorescent piezoelectric sensor comprises the following steps:

[0046] (1) Preparation of PVDF-HFP solution: N,N-dimethylformamide and acetone were mixed and stirred at a mass ratio of 1:0.8 for 10 min to obtain solution a; then PVDF-HFP and solution a were mixed and stirred at a mass ratio of 1:5.6 for 4 h to obtain PVDF-HFP solution;

[0047] (2) Preparation of CQDs suspension: CQDs and water were mixed at a mass ratio of 1:15 and ultrasonicated for 40 min to obtain a CQDs suspension;

[0048] (3) Preparation of functional composite film: The conductive surface of the ITO-PEN electrode was treated with oxygen plasma for 10 min, and then the PVDF-HFP solution was spin-coated on the conductive surface of the ITO-PEN electrode. After standing at room temperature for 60 min, the surface was kept at 100°C for 1.5 h to form a PVDF-HFP piezoelectric layer. Subsequently, the CQDs suspension was spin-coated on the PVDF-HFP piezoelectric layer and kept at 110°C for 1.5 h to form a CQDs fluorescent layer. Finally, the PVDF-HFP solution was spin-coated on the CQDs fluorescent layer again. After standing at room temperature for 60 min, the surface was kept at 100°C for 1.5 h to form a PVDF-HFP piezoelectric layer. An ITO-PEN electrode with a functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer was obtained. The coating thicknesses of the PVDF-HFP piezoelectric layer and the CQDs fluorescent layer were 20 µm and 40 µm, respectively.

[0049] (4) Sensor assembly: Place the ITO-PEN electrode with the functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited above with one side facing up, and then take another blank ITO-PEN electrode with the conductive surface facing down and cover its upper surface in an offset manner. The uncovered parts of the two electrodes are used as leads, which are fixed by coating silicone around them. The wires are fixed to the leads of the two electrodes by conductive silver paste, thus obtaining a flexible fluorescent piezoelectric sensor; wherein the overlapping part of the two electrodes accounts for 75% of the surface area of ​​a single electrode.

[0050] Example 3

[0051] A method for preparing a flexible fluorescent piezoelectric sensor comprises the following steps:

[0052] (1) Preparation of PVDF-HFP solution: N,N-dimethylformamide and acetone were mixed and stirred at a mass ratio of 1:0.4 for 30 min to obtain solution a; then PVDF-HFP and solution a were mixed and stirred at a mass ratio of 1:8.5 for 3 h to obtain PVDF-HFP solution;

[0053] (2) Preparation of CQDs suspension: CQDs and water were mixed at a mass ratio of 1:8 and ultrasonicated for 90 min to obtain a CQDs suspension;

[0054] (3) Preparation of functional composite film: The conductive surface of the ITO-PEN electrode was treated with oxygen plasma for 15 minutes, and then the PVDF-HFP solution was spin-coated on the conductive surface of the ITO-PEN electrode. After standing at room temperature for 90 minutes, it was kept at 120°C for 1 hour to form a PVDF-HFP piezoelectric layer. Subsequently, the CQDs suspension was spin-coated on the PVDF-HFP piezoelectric layer and kept at 110°C for 2 hours to form a CQDs fluorescent layer. Finally, the PVDF-HFP solution was spin-coated on the CQDs fluorescent layer again, and after standing at room temperature for 90 minutes, it was kept at 120°C for 1 hour to form a PVDF-HFP piezoelectric layer. An ITO-PEN electrode with a functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer was obtained. The coating thicknesses of the PVDF-HFP piezoelectric layer and the CQDs fluorescent layer were 40µm and 20µm, respectively.

[0055] (4) Sensor assembly: Place the ITO-PEN electrode with the functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited above with one side facing up, and then take another blank ITO-PEN electrode with the conductive surface facing down and cover its upper surface in an offset manner. The uncovered parts of the two electrodes are used as leads, which are fixed by coating silicone around them. The wires are fixed to the leads of the two electrodes by conductive silver paste, thus obtaining a flexible fluorescent piezoelectric sensor; wherein the overlapping part of the two electrodes accounts for 75% of the surface area of ​​a single electrode.

[0056] Example 4

[0057] A method for preparing a flexible fluorescent piezoelectric sensor comprises the following steps:

[0058] (1) Preparation of PVDF-HFP solution: N,N-dimethylformamide and acetone were mixed and stirred at a mass ratio of 1:1 for 15 minutes to obtain solution a; then PVDF-HFP and solution a were mixed and stirred at a mass ratio of 1:10 for 2 hours to obtain PVDF-HFP solution;

[0059] (2) Preparation of CQDs suspension: CQDs and water were mixed at a mass ratio of 1:18 and ultrasonicated for 120 min to obtain a CQDs suspension;

[0060] (3) Preparation of functional composite film: The conductive surface of the ITO-PEN electrode was treated with oxygen plasma for 8 minutes, and then the PVDF-HFP solution was spin-coated on the conductive surface of the ITO-PEN electrode, and then the surface was kept at room temperature for 120 minutes and then kept at 115°C for 2 hours to form a PVDF-HFP piezoelectric layer. Subsequently, the CQDs suspension was spin-coated on the PVDF-HFP piezoelectric layer and kept at 115°C for 2 hours to form a CQDs fluorescent layer. Finally, the PVDF-HFP solution was spin-coated on the CQDs fluorescent layer again, and then the surface was kept at room temperature for 120 minutes and then kept at 115°C for 2 hours to form a PVDF-HFP piezoelectric layer. An ITO-PEN electrode with a functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer was obtained. The coating thicknesses of the PVDF-HFP piezoelectric layer and the CQDs fluorescent layer were 25µm and 35µm, respectively.

[0061] (4) Sensor assembly: Place the ITO-PEN electrode with the functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited above with one side facing up, and then take another blank ITO-PEN electrode with the conductive surface facing down and cover its upper surface in an offset manner. The uncovered parts of the two electrodes are used as leads, which are fixed by coating silicone around them. The wires are fixed to the leads of the two electrodes by conductive silver paste, thus obtaining a flexible fluorescent piezoelectric sensor; wherein the overlapping part of the two electrodes accounts for 75% of the surface area of ​​a single electrode.

[0062] Example 5

[0063] A method for preparing a flexible fluorescent piezoelectric sensor comprises the following steps:

[0064] (1) Preparation of PVDF-HFP solution: N,N-dimethylformamide and acetone were mixed and stirred at a mass ratio of 1:0.75 for 25 min to obtain solution a; then PVDF-HFP and solution a were mixed and stirred at a mass ratio of 1:6.43 for 2.5 h to obtain PVDF-HFP solution;

[0065] (2) Preparation of CQDs suspension: CQDs and water were mixed at a mass ratio of 1:5 and ultrasonicated for 30 min to obtain a CQDs suspension;

[0066] (3) Preparation of functional composite film: The conductive surface of the ITO-PEN electrode was treated with oxygen plasma for 13 minutes, and then the PVDF-HFP solution was spin-coated on the conductive surface of the ITO-PEN electrode, and then the solution was kept at room temperature for 100 minutes and then kept at 110°C for 1 hour to form a PVDF-HFP piezoelectric layer. Subsequently, the CQDs suspension was spin-coated on the PVDF-HFP piezoelectric layer and kept at 100°C for 2 hours to form a CQDs fluorescent layer. Finally, the PVDF-HFP solution was spin-coated on the CQDs fluorescent layer again, and then the solution was kept at room temperature for 100 minutes and then kept at 110°C for 1 hour to form a PVDF-HFP piezoelectric layer. An ITO-PEN electrode with a functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer was obtained. The coating thicknesses of the PVDF-HFP piezoelectric layer and the CQDs fluorescent layer were 30 µm and 30 µm, respectively.

[0067] (4) Sensor assembly: Place the ITO-PEN electrode with the functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited above with one side facing up, and then take another blank ITO-PEN electrode with the conductive surface facing down and cover its upper surface in an offset manner. The uncovered parts of the two electrodes are used as leads, which are fixed by coating silicone around them. The wires are fixed to the leads of the two electrodes by conductive silver paste, thus obtaining a flexible fluorescent piezoelectric sensor; wherein the overlapping part of the two electrodes accounts for 75% of the surface area of ​​a single electrode.

[0068] Figure 2 This is the fluorescence spectrum of the flexible fluorescent piezoelectric sensor in Example 1, which shows that the flexible fluorescent piezoelectric sensor exhibits relatively excellent fluorescence performance, and its fluorescence emission intensity peak is around 550nm wavelength, corresponding to the green light band in visible light.

[0069] Figure 3 This is a macroscopic photograph of the flexible fluorescent piezoelectric sensor in Example 1 under the excited fluorescent state. It can be seen that the flexible fluorescent piezoelectric sensor has excellent fluorescence, and the color of the fluorescence is blue-green under the excitation of ultraviolet light.

[0070] Figure 4 This is the real-time output voltage-time curve of the flexible fluorescent piezoelectric sensor in Example 1 under periodic constant force. It can be seen that under periodic constant force, the real-time output voltage of the flexible fluorescent piezoelectric sensor has complete periodicity and also has self-powered working characteristics.

[0071] Figure 5is the real-time output voltage-force curve of the flexible fluorescent piezoelectric sensor in Example 1. When the applied external force increases from 0.6959 N to 3.3516 N, the real-time output voltage of the sensor increases from 0.22 V to 1.06 V, showing an excellent linear relationship, that is, R 2 > 0.966, the sensitivity of the flexible fluorescent piezoelectric sensor reached 0.321V / N.

Claims

1. A method for preparing a flexible fluorescent piezoelectric sensor, comprising the following steps: (1) Preparation of PVDF-HFP solution: N,N-dimethylformamide and additive were mixed and stirred at a mass ratio of 1: (0.2-1) for 10-30 min to obtain solution a; then PVDF-HFP and solution a were mixed and stirred at a mass ratio of 1: (5-10) for 2-4 h to obtain PVDF-HFP solution; (2) Preparation of CQDs suspension: CQDs and water were mixed in a mass ratio of 1:(5-20) and ultrasonicated for 30-120 min to obtain a CQDs suspension; (3) Preparation of functional composite film: The conductive surface of the ITO-PEN electrode is treated with oxygen plasma, and then the PVDF-HFP solution is coated on the conductive surface of the ITO-PEN electrode, and a PVDF-HFP piezoelectric layer is formed by heat treatment. Subsequently, a CQDs suspension is coated on the PVDF-HFP piezoelectric layer, and a CQDs fluorescent layer is formed by drying. Finally, the PVDF-HFP solution is coated on the CQDs fluorescent layer again, and a PVDF-HFP piezoelectric layer is formed by heat treatment, thereby obtaining an ITO-PEN electrode with a functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited on one side; (4) Sensor assembly: Place the ITO-PEN electrode with the functional composite film of PVDF-HFP piezoelectric layer / CQDs fluorescent layer / PVDF-HFP piezoelectric layer deposited above with one side facing up, and then take another blank ITO-PEN electrode with the conductive surface facing down, and cover its upper surface in an offset manner. The uncovered parts of the two electrodes are used as leads, and silicone is coated around them for fixation. The wires are fixed to the leads of the two electrodes by conductive silver paste, thus obtaining a flexible fluorescent piezoelectric sensor.

2. The method for preparing the flexible fluorescent piezoelectric sensor according to claim 1, characterized in that: The steps include: In step (1), the additive is one or more of acetone, ethanol, methyl ethyl ketone, and ethyl acetate.

3. The method for preparing the flexible fluorescent piezoelectric sensor according to claim 1, characterized in that: In step (3), the oxygen plasma treatment time is 5 to 15 minutes.

4. The method for preparing the flexible fluorescent piezoelectric sensor according to claim 1, characterized in that: In step (3), coating is carried out by any one of spin coating, scraper coating, screen printing and casting.

5. The method for preparing the flexible fluorescent piezoelectric sensor according to claim 1, characterized in that: In step (3), the coating thicknesses of the PVDF-HFP piezoelectric layer and the CQDs fluorescent layer are 10~50µm and 10~50µm, respectively.

6. The method for preparing the flexible fluorescent piezoelectric sensor according to claim 1, characterized in that: In step (3), the specific steps of heat treatment are: first standing at room temperature for 30 to 120 minutes, and then keeping warm at 100 to 120°C for 1 to 2 hours.

7. The method for preparing a flexible fluorescent piezoelectric sensor according to claim 1, characterized in that: In step (3), the specific steps of drying are: keeping warm at 100-120°C for 1-2 hours.

8. The method for preparing a flexible fluorescent piezoelectric sensor according to claim 1, characterized in that: In step (4), the overlapping portion of the two electrodes accounts for 70-80% of the surface area of ​​a single electrode.

9. A flexible fluorescent piezoelectric sensor, prepared according to any one of the preparation methods of claims 1 to 8.