Dual-band quantum dot layers, devices, their fabrication methods and applications
By introducing a dual-band quantum dot layer into the detection device and utilizing the unidirectional PN heterojunction structure, the problem of requiring different bias voltages in the prior art is solved, enabling simultaneous detection of infrared and visible light under the same bias voltage, thereby improving photoelectric conversion efficiency and detection efficiency.
Patent Information
- Application Number
- CN202211311307.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-10-25
AI Technical Summary
Existing dual-band detection devices require different bias voltages to be set according to the detection band, and cannot detect infrared and visible light simultaneously under the same bias voltage, making their use conditions very demanding.
A dual-band quantum dot layer is used, comprising an infrared photosensitive film layer and a visible light photosensitive film layer, forming two co-directional PN heterojunctions. These are composed of a chalcogenide silver quantum dot doping layer, a chalcogenide mercury quantum dot intrinsic layer, a cadmium telluride quantum dot layer, and a zinc oxide electron transport layer, respectively. The detection device is fabricated through coating and vapor deposition methods.
It achieves simultaneous detection of infrared and visible light under the same bias voltage, with high photoelectric conversion efficiency and good detection efficiency.
Smart Images

Figure CN115692523B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an infrared detector, belonging to the field of optoelectronic sensor technology, specifically to a dual-band quantum dot layer, device, its fabrication method, and its application. Background Technology
[0002] The development of information fusion technology has made it possible for multiple sensors to work collaboratively. Information fusion technology refers to the multi-level, multi-faceted, and multi-layered processing and fusion of information acquired from the same scene at the same time, thereby obtaining more reliable, richer, more accurate, and more meaningful information. The coupling of visible light detectors and infrared detectors is currently one of the most common information fusion technologies. Visible light detectors can capture detailed information about the object being measured and have high spatial resolution, but because they operate within an atmospheric window, they are highly susceptible to weather conditions and cannot operate in all weather. Furthermore, visible light images cannot detect targets hidden in complex backgrounds. Short-wave infrared detectors, on the other hand, utilize blackbody radiation for imaging, are less affected by lighting conditions and adverse weather, and have nighttime imaging capabilities. However, due to limitations in their imaging principles, infrared images have low contrast, strong spatial correlation, and poor detail reproduction, resulting in imaging effects that do not conform to human visual perception. Coupled with visible light detectors and infrared detectors, the shortcomings of each imaging system can be compensated for, leveraging the advantages of both visible light and infrared detection. This allows the detector to possess the advantages of both, improving the system's detection and reconnaissance capabilities.
[0003] Chinese invention patent application (application number: 2022107534911, application date: 2022-06-30) discloses a non-flip-bonded dual-band quantum dot pixel and focal plane array. The focal plane array utilizes the semiconductor compound properties of CdTe and ZnO and is fabricated using a non-flip-bonded technology. The resulting dual-band detector has the advantages of high photoelectric conversion efficiency and good device efficiency. However, in practical use, this dual-band detector requires different bias voltages to be set according to the detection band, and cannot achieve simultaneous detection of infrared and visible light under the same bias voltage. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention discloses a dual-band quantum dot layer, a device, its fabrication method, and its applications. This device enables simultaneous detection of infrared and visible light under the same bias voltage, and exhibits high photoelectric conversion efficiency and good detection efficiency.
[0005] To achieve the above technical objectives, the present invention discloses a dual-band quantum dot layer, wherein the quantum dot layer comprises an infrared photosensitive film layer and a visible light photosensitive film layer composited together, and the infrared photosensitive film layer and the visible light photosensitive film layer constitute two co-directional PN heterojunctions.
[0006] Furthermore, the infrared photosensitive film layer is composed of a chalcogenide silver quantum dot doped layer and a chalcogenide mercury quantum dot intrinsic layer, and the chalcogenide silver quantum dot doped layer and the chalcogenide mercury quantum dot intrinsic layer form a PN heterojunction;
[0007] The visible light photosensitive film layer is composed of a zinc oxide electron transport layer and a cadmium telluride quantum dot layer, and the cadmium telluride quantum dot layer and the zinc oxide electron transport layer form the remaining PN heterojunction.
[0008] Furthermore, the thickness of the chalcogenide silver quantum dot doped layer is less than the thickness of the chalcogenide mercury quantum dot intrinsic layer.
[0009] As an optional embodiment of the present invention, the thickness of the chalcogenide silver quantum dot doped layer is 5-15 nm, preferably 8-12 nm, and most preferably 10 nm.
[0010] The thickness of the intrinsic layer of the chalcogenide mercury quantum dots is 300–600 nm, preferably 450–550 nm, and most preferably 500 nm.
[0011] Furthermore, the material of the chalcogenide silver quantum dot doped layer is any one of silver sulfide, silver selenide, and silver telluride, with silver telluride being preferred;
[0012] Furthermore, the intrinsic material of the chalcogenide mercury quantum dot layer is any one of mercury sulfide, mercury selenide, and mercury telluride, with mercury telluride being preferred.
[0013] Furthermore, the thickness of the zinc oxide electron transport layer is less than the thickness of the cadmium telluride quantum dot layer.
[0014] As an optional embodiment of the present invention, the thickness of the zinc oxide electron transport layer is 5-15 nm, preferably 8-12 nm, and most preferably 10 nm.
[0015] The thickness of the cadmium telluride quantum dot layer is 300–600 nm, preferably 450–550 nm, and most preferably 500 nm.
[0016] Furthermore, the thickness between the infrared photosensitive film layer and the visible light photosensitive film layer satisfies the following condition: when the thickness of the infrared photosensitive film layer is greater than the thickness of the visible light photosensitive film layer, the infrared photosensitive ability is stronger; conversely, the visible light photosensitive ability is stronger.
[0017] As an optional embodiment of the present invention, the present invention discloses a dual-band quantum dot layer, the dual-band quantum dot layer comprising:
[0018] Silver telluride quantum dot doping layers arranged sequentially from top to bottom;
[0019] Intrinsic layer of mercury telluride quantum dots;
[0020] Cadmium telluride quantum dot layer;
[0021] Zinc oxide electron transport layer;
[0022] The silver telluride quantum dot doping layer and the mercury telluride quantum dot intrinsic layer form a PN heterojunction, and the cadmium telluride quantum dot layer and the zinc oxide electron transport layer form the remaining PN heterojunction. The two PN heterojunctions are arranged in the same direction.
[0023] A second objective of this invention is to provide a detection device comprising at least one pixel, the pixel comprising: a substrate layer, at least one dual-band quantum dot layer as described in the first aspect, and a top electrode layer, arranged sequentially from bottom to top.
[0024] Further, the substrate layer is made of an infrared transparent conductive material laminated on a sapphire substrate or a silicon substrate, wherein the infrared transparent conductive material includes ITO, FTO, or AZO laminated on the sapphire substrate or the silicon substrate. Preferably, the infrared transparent conductive material is ITO laminated on a sapphire substrate. Preferably, the lamination is performed by physical deposition, and the physical deposition is magnetron sputtering.
[0025] As an optional embodiment of the present invention, the thickness of the infrared transparent conductive material is 40-60 nm, preferably 50 nm.
[0026] Furthermore, the top electrode layer is made of a metallic conductive material, which is any one of gold, silver, copper, or aluminum. Preferably, the metallic conductive material is gold.
[0027] As an optional embodiment of the present invention, the thickness of the metallic conductive material is 30-50 nm, preferably 40 nm.
[0028] Furthermore, the detector includes a plurality of pixels, which are arranged in a row and column array.
[0029] As an optional embodiment of the present invention, the detection device is a focal plane array device, which includes a readout circuit and pixels arranged in a row and column array on the readout circuit.
[0030] As an optional embodiment of the present invention, the focal plane array device includes:
[0031] The readout circuits are arranged sequentially from bottom to top;
[0032] Zinc oxide electron transport layer;
[0033] Cadmium telluride quantum dot layer;
[0034] Intrinsic layer of mercury telluride quantum dots;
[0035] Silver telluride quantum dot doped layer;
[0036] Top electrode layer;
[0037] The fabrication process of the readout circuit includes the arrangement of a substrate layer.
[0038] The third objective of this invention is to disclose a method for fabricating a detector device, wherein the method includes sequentially laminating a visible light photosensitive film layer, an infrared photosensitive film layer, and a top electrode layer on the surface of a substrate layer, wherein the infrared photosensitive film layer and the visible light photosensitive film layer constitute two co-directional PN heterojunctions.
[0039] Furthermore, the composite is a coating method, which includes one or more of the following: drop coating, spray coating, spin coating, knife coating, or ink printing, with spin coating being preferred.
[0040] As an optional embodiment of the present invention, a method for preparing a detection device includes the following steps:
[0041] (1) Indium tin oxide is physically deposited on the surface of a sapphire substrate to form a substrate layer.
[0042] (2) A ZnO solution is coated on the surface of the substrate layer. The ZnO solution is ZnO dissolved in isopropanol. The concentration of the ZnO solution is 15-25 mg / mL, preferably 20 mg / mL. Then, the substrate is annealed on a hot plate at 80°C for a period of time to obtain a zinc oxide electron transport layer.
[0043] (3) Coat the zinc oxide electron transport layer with the cadmium telluride quantum dot ink, then place it on a hot plate at 60°C for a period of time, then place it in a saturated CdCl2 solution, which is a saturated methanol solution of CdCl2. Next, rinse off the excess CdCl2 solution with IPA, and finally place it on a hot plate at 350°C for sintering. Repeat step (3) 8 to 12 times to obtain the cadmium telluride quantum dot layer.
[0044] (4) Coat the surface of the cadmium telluride quantum dot layer with the mercury telluride quantum dot ink, then drop EDT onto the coating layer for a period of time, rinse the residual EDT with IPA, then drop HgCl2 solution onto the coating layer, rinse the residual HgCl2 with IPA, and use a spin coater to remove excess IPA. Repeat step (4) 8 to 12 times to obtain the intrinsic layer of mercury telluride quantum dots. The HgCl2 solution is a methanol solution of any concentration of HgCl2.
[0045] (5) Coat the surface of the intrinsic layer of mercury telluride quantum dot with the silver telluride quantum dot ink, then add HgCl2 solution for treatment, rinse the residual HgCl2 with IPA to prepare the silver telluride quantum dot doped layer, wherein the HgCl2 solution is a methanol solution of HgCl2 of any concentration.
[0046] (6) A top electrode layer is formed by vapor deposition of gold on the surface of the silver telluride quantum dot doped layer. The vapor deposition is performed by evaporation.
[0047] As an optional embodiment of the present invention, the preparation method of the cadmium telluride quantum dot ink is as follows:
[0048] (1) Preparation of thermal equilibrium solution:
[0049] Cadmium oxide is placed in a reaction vessel, and oleic acid and octadecene are added. The reaction vessel is kept in an inert environment. The temperature of the reaction vessel is initially set to 220°C while stirring. After the solution in the vessel becomes clear, the temperature is raised to 270°C and allowed to reach thermal equilibrium for half an hour. The preferred molar volume ratio of oleic acid, octadecene, and cadmium oxide is 15 mmol: 18.8 ml: 20.3 ml. The inert environment is an inert gas protective condition.
[0050] (2) Preparation of TBP-Te solution:
[0051] At room temperature, tellurium powder was dissolved in tributyl phosphate in a glove box and stirred until the solution turned bright yellow. The solution was then removed from the glove box to obtain a TBP-Te solution.
[0052] The preferred molar ratio of cadmium oxide to tellurium powder is 1:1.
[0053] (3) Synthetic cadmium telluride quantum dot ink:
[0054] The thermal equilibrium solution from step (1) is rapidly injected into the TBP-Te solution from step (2). After the injection is complete, the solution is cooled for a long time with an air gun, and then cooled in a water bath. A mixture of toluene and anhydrous ethanol is added to the obtained mixture and centrifuged twice. The centrifuged material is then redissolved in a mixture of pyridine and n-propanol to obtain cadmium telluride quantum dot ink. This cadmium telluride quantum dot ink is stable and can be stored in a glove box for a period of time.
[0055] The volume ratio of toluene to anhydrous ethanol is (1-2):(2-4), preferably 1:2;
[0056] The volume ratio of pyridine to n-propanol is (1-2):(2-4), preferably 1:2.
[0057] As an optional embodiment of the present invention, the preparation method of the mercury telluride quantum dot ink is as follows:
[0058] (1.1) TOP-Te solution: Te particles are dispersed in tri-n-octylphosphine in an inert environment to form a bright yellow solution, which is called TOP-Te solution; the inert environment is preferably a nitrogen glove box, and the dispersion is preferably stirred; the molar ratio of Te particles to tri-n-octylphosphine is preferably 1:1;
[0059] (1.2) Thermal equilibrium solution: Mercuric chloride is added to oleylamine in an inert environment and heated to 100°C to form a transparent, pale yellow solution; the heating is preferably a heating plate with magnetic stirring function, and the inert environment is preferably a nitrogen glove box; the molar volume ratio of mercuric chloride to oleylamine is 0.1 mmol: 4 mL.
[0060] (1.3) Quenching solution: Mix tri-n-octylphosphine and trichloroethylene and place them in a reaction vessel. Store at low temperature. The volume ratio of tri-n-octylphosphine to trichloroethylene is 0.5 mL: 4 mL. It is preferable to store at low temperature in a refrigerator.
[0061] (1.4) Synthesis of HgTe quantum dot ink using hot injection method: In an inert environment, the thermal equilibrium solution from step (1.2) is brought to thermal equilibrium with the temperature required for the reaction, generally 80℃~100℃. The TOP-Te solution from step (1.1) is then rapidly added, and the reaction time is set, generally 4min~10min. After the reaction is complete, the quenching solution from (1.3) is added to cool the reaction. The ink is then removed from the inert environment and cooled to obtain mercury telluride quantum dot ink. Preferably, the inert environment is a glove box, the cooling is a water bath, the drying is a nitrogen gun, and the centrifugal precipitation is carried out in a centrifuge.
[0062] Generally, the higher the reaction temperature and the longer the reaction time, the larger the quantum dot and the longer the absorption wavelength. Different temperatures and reaction times control the size of the quantum dot, i.e. the cutoff wavelength of absorption, and ultimately achieve a short-wave range of 1.5 to 2.5 μm and a medium-wave range of 3 to 5 μm.
[0063] As an optional embodiment of the present invention, the preparation method of the silver telluride quantum dot ink is as follows:
[0064] Silver nitrate was dissolved in oleylamine and oleic acid, and stirred at 70°C for 30 min in a nitrogen glove box to obtain a reaction solution; the preferred molar volume ratio of silver nitrate to oleylamine and oleic acid was 0.2 mmol: 5 mL: 0.5 mL.
[0065] Tellurium particles were dissolved in TOP and heated to 160°C. When the temperature exceeded 140°C, the solution began to turn yellow. The solution was kept at 160°C for 35–45 minutes until it turned into orange TOP-Te. The molar ratio of silver nitrate to tellurium particles was 2:1, and the molar volume ratio of tellurium particles to TOP was 0.1 mmol:0.5 mL.
[0066] When TOP-Te is injected into the reaction solution, the solution immediately turns from orange to black. The reaction time is 10 minutes. After cooling, the solution is stored in a refrigerator.
[0067] The fourth objective of this invention is to disclose the application of a dual-band quantum dot layer as described in the first aspect, or a detector device as described in the second aspect, or a detector device prepared by the method described in the third aspect, in visible light (390–760 nm) and infrared light (1.5–5 μm).
[0068] As an optional embodiment of the present invention, the detection device is used in the visible light range of 390–760 nm and the infrared range of 1.5–3 μm, preferably in the range of 1.5–2.5 μm.
[0069] As an optional embodiment of the present invention, the detector is used in visible light (390–760 nm) and infrared light (3–5 μm).
[0070] The technical solution provided by the embodiments of the present invention has the following advantages compared with the prior art:
[0071] The dual-band detector device prepared by this invention can simultaneously detect infrared and visible light under the same bias voltage, and the device has high photoelectric conversion efficiency and good detection efficiency. Attached Figure Description
[0072] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0073] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0074] Figure 1 This is a schematic diagram of the structure of the dual-band quantum dot layer designed in this invention;
[0075] Figure 2 This is a schematic diagram of the structure of the dual-band detector device designed for this invention;
[0076] Figure 3The spectral absorption curve of cadmium telluride was prepared for the embodiments of the present invention;
[0077] Figure 4 The absorption spectrum of mercury telluride was prepared for an embodiment of the present invention;
[0078] Figure 5 The band structure diagram of the dual-band detector device prepared according to an embodiment of the present invention;
[0079] Figure 6 The spectral response curves of the dual-band detector device prepared for embodiments of the present invention;
[0080] The component numbers in the above-mentioned attached diagram are as follows:
[0081] 101. Infrared photosensitive film layer; 102. Visible light photosensitive film layer; 103. Top electrode layer; 104. Substrate layer;
[0082] 101-1, Chalcogenide silver quantum dot doped layer;
[0083] 101-2, Intrinsic layer of chalcogenide mercury quantum dots;
[0084] 102-1, Cadmium telluride quantum dot layer;
[0085] 102-2, Zinc oxide electron transport layer. Detailed Implementation
[0086] To better understand the above-mentioned objectives, features, and advantages of the present invention, the solutions of the present invention will be further described below. It should be noted that, unless otherwise specified, the embodiments of the present invention and the features thereof can be combined with each other.
[0087] The names and abbreviations of the compounds involved in this invention are as follows:
[0088] Te: Tellurium; OAM: Oleamine; OA: Oleic acid; ODE: Octadecylene; TBP: Tributyl phosphate; TBP-Te: Tributyl phosphate mixture of tellurium; TOP: Tri-n-octylphosphine; TOP-Te: Tri-n-octylphosphine mixture of tellurium; TCE: Trichloroethylene; HgCl2: Mercuric chloride; HgTe: Mercuric telluride; Ag2Te: Silver telluride; CdTe: Cadmium telluride; CdO: Cadmium oxide; CdCl2: Cadmium chloride; ZnO: Zinc oxide; Al2O3: Aluminum oxide; TCE: Tetrachloroethylene; IPA: Isopropanol; EDT: Ethylene dithiol; ITO: Indium tin oxide; FTO: Fluorine-doped tin dioxide; AZO: Aluminum-doped zinc oxide.
[0089] This invention addresses the technical problem of existing dual-band detection devices requiring separate bias voltages for each detection band, resulting in stringent operating conditions and inconvenience. It provides a dual-band quantum dot layer, device, its fabrication method, and its applications. This device enables simultaneous detection of infrared and visible light under the same bias voltage, exhibiting high photoelectric conversion efficiency and good detection efficiency.
[0090] To achieve the aforementioned technical objectives, the present invention provides a dual-band quantum dot layer, wherein the quantum dot layer comprises an infrared photosensitive film layer 101 and a visible light photosensitive film layer 102 composited together, the infrared photosensitive film layer 101 and the visible light photosensitive film layer 102 forming two co-directional PN heterojunctions. The structure of the dual-band quantum dot layer is as follows: Figure 1 As shown. Furthermore, any relationship between the thickness of the infrared photosensitive film layer and the thickness of the visible light photosensitive film layer is within the protection scope of this invention.
[0091] In some embodiments, the infrared photosensitive film layer 101 is composed of a chalcogenide silver quantum dot doped layer 101-1 and a chalcogenide mercury quantum dot intrinsic layer 101-2, and the visible light photosensitive film layer 102 is composed of a cadmium telluride quantum dot layer 102-1 and a zinc oxide electron transport layer 102-2.
[0092] In some embodiments, the thickness of the chalcogenide silver quantum dot doped layer is less than the thickness of the chalcogenide mercury quantum dot intrinsic layer.
[0093] In some embodiments, the thickness of the chalcogenide silver quantum dot doped layer is 5–15 nm, preferably 8–12 nm, and most preferably 10 nm.
[0094] In some embodiments, the thickness of the intrinsic layer of the chalcogenide mercury quantum dots is 300–600 nm, preferably 450–550 nm, and most preferably 500 nm.
[0095] For example, the thickness of the chalcogenide silver quantum dot doped layer can be 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, or 15nm.
[0096] For example, the thickness of the intrinsic layer of the sulfide mercury quantum dot can be 300nm, 320nm, 340nm, 360nm, 380nm, 400nm, 420nm, 440nm, 460nm, 480nm, 500nm, 520nm, 540nm, 560nm, 580nm, or 600nm.
[0097] In some embodiments, the material of the chalcogenide silver quantum dot doped layer is any one of silver sulfide, silver selenide, and silver telluride, with silver telluride being preferred.
[0098] In some embodiments, the intrinsic material of the chalcogenide mercury quantum dot layer is any one of mercury sulfide, mercury selenide, and mercury telluride, with mercury telluride being preferred.
[0099] In some embodiments, the thickness of the zinc oxide electron transport layer is less than the thickness of the cadmium telluride quantum dot layer.
[0100] In some embodiments, the thickness of the zinc oxide electron transport layer is 5–15 nm, preferably 8–12 nm, and most preferably 10 nm.
[0101] For example, the thickness of the zinc oxide electron transport layer can be 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, or 15nm.
[0102] In some embodiments, the thickness of the cadmium telluride quantum dot layer is 300–600 nm, preferably 450–550 nm, and most preferably 500 nm.
[0103] For example, the thickness of the cadmium telluride quantum dot layer can be 300nm, 320nm, 340nm, 360nm, 380nm, 400nm, 420nm, 440nm, 460nm, 480nm, 500nm, 520nm, 540nm, 560nm, 580nm, or 600nm.
[0104] In some embodiments, the thickness between the infrared photosensitive film layer and the visible light photosensitive film layer satisfies the following condition: when the thickness of the infrared photosensitive film layer is greater than the thickness of the visible light photosensitive film layer, the infrared photosensitive layer is stronger; conversely, the visible light photosensitive layer is stronger when the thickness of the infrared photosensitive film layer is less than the thickness of the visible light photosensitive film layer.
[0105] For example, the present invention discloses a dual-band quantum dot layer, the dual-band quantum dot layer comprising:
[0106] Silver telluride quantum dot doping layers arranged sequentially from top to bottom;
[0107] Intrinsic layer of mercury telluride quantum dots;
[0108] Cadmium telluride quantum dot layer;
[0109] Zinc oxide electron transport layer;
[0110] The silver telluride quantum dot doping layer and the mercury telluride quantum dot intrinsic layer form a PN heterojunction, and the cadmium telluride quantum dot layer and the zinc oxide electron transport layer form the remaining PN heterojunction. The two PN heterojunctions are arranged in the same direction.
[0111] A second aspect of the present invention is to provide a detection device comprising at least one pixel, the pixel comprising: a substrate layer 104 disposed from bottom to top, at least one dual-band quantum dot layer 101, 102 and a top electrode layer 103 as described in the first aspect.
[0112] In some embodiments, the substrate layer is made of an infrared-transparent conductive material laminated on a sapphire substrate or a silicon substrate, wherein the infrared-transparent conductive material includes ITO, FTO, or AZO laminated on the sapphire substrate or the silicon substrate. Preferably, the infrared-transparent conductive material is ITO laminated on a sapphire substrate. Preferably, the lamination is performed by physical deposition, and the physical deposition is magnetron sputtering.
[0113] In some embodiments, the thickness of the infrared transparent conductive material is 40–60 nm, preferably 50 nm.
[0114] In some embodiments, the top electrode layer is made of a metallic conductive material, which is any one of gold, silver, copper, or aluminum. Preferably, the metallic conductive material is gold.
[0115] In some embodiments, the thickness of the metallic conductive material is 30-50 nm, preferably 40 nm.
[0116] In some embodiments, the detector includes a plurality of pixels arranged in a row and column array.
[0117] For example, the thickness of the infrared transparent conductive material is 40nm, 45nm, 50nm, 55nm, or 60nm.
[0118] For example, the thickness of the metallic conductive material is 30nm, 35nm, 40nm, 45nm, or 50nm.
[0119] For example, the present invention provides a focal plane array device, the focal plane array device comprising:
[0120] The readout circuits are arranged sequentially from bottom to top;
[0121] Zinc oxide electron transport layer;
[0122] Cadmium telluride quantum dot layer;
[0123] Intrinsic layer of mercury telluride quantum dots;
[0124] Silver telluride quantum dot doped layer;
[0125] Top electrode layer;
[0126] The fabrication process of the readout circuit includes the arrangement of a substrate layer, which is a prior art and will not be described in detail in this invention.
[0127] A third aspect of the present invention is to provide a method for fabricating a detector device, the method comprising sequentially laminating a visible light photosensitive film layer, an infrared photosensitive film layer and a top electrode layer on the surface of a substrate layer, wherein the infrared photosensitive film layer and the visible light photosensitive film layer constitute two co-directional PN heterojunctions.
[0128] In some embodiments, the composite is a coating method, which includes one or more of the following: drop coating, spray coating, spin coating, knife coating, or ink printing, with spin coating being preferred.
[0129] For example, the present invention discloses a method for fabricating a detection device, the method comprising the following steps:
[0130] (1) Indium tin oxide is physically deposited on the surface of a sapphire substrate to form a substrate layer.
[0131] (2) A ZnO solution is coated on the surface of the substrate layer. The ZnO solution is ZnO dissolved in isopropanol. The concentration of the ZnO solution is 15-25 mg / mL, preferably 20 mg / mL. Then, the substrate is annealed on a hot plate at 80°C for a period of time to obtain a zinc oxide electron transport layer.
[0132] (3) Coat the zinc oxide electron transport layer with the cadmium telluride quantum dot ink, then place it on a hot plate at 60°C for a period of time, then place it in a saturated CdCl2 solution, which is a saturated methanol solution of CdCl2. Next, rinse off the excess CdCl2 solution with IPA, and finally place it on a hot plate at 350°C for sintering. Repeat step (3) 8 to 12 times to obtain the cadmium telluride quantum dot layer.
[0133] (4) Coat the surface of the cadmium telluride quantum dot layer with the mercury telluride quantum dot ink, then drop EDT onto the coating layer for a period of time, rinse the residual EDT with IPA, then drop HgCl2 solution onto the coating layer, rinse the residual HgCl2 with IPA, and use a spin coater to remove excess IPA. Repeat step (4) 8 to 12 times to obtain the intrinsic layer of mercury telluride quantum dots. The HgCl2 solution is a methanol solution of any concentration of HgCl2.
[0134] (5) Coat the surface of the intrinsic layer of mercury telluride quantum dot with the silver telluride quantum dot ink, then add HgCl2 solution for treatment, rinse the residual HgCl2 with IPA to prepare the silver telluride quantum dot doped layer, wherein the HgCl2 solution is a methanol solution of HgCl2 of any concentration.
[0135] (6) A top electrode layer is formed by vapor deposition of gold on the surface of the silver telluride quantum dot doped layer. The vapor deposition is performed by evaporation.
[0136] In some embodiments, the cadmium telluride quantum dot ink is prepared as follows:
[0137] (1) Preparation of thermal equilibrium solution:
[0138] Cadmium oxide is placed in a reaction vessel, and oleic acid and octadecene are added. The reaction vessel is kept in an inert environment. The temperature of the reaction vessel is initially set to 220°C while stirring. After the solution in the vessel becomes clear, the temperature is raised to 270°C and allowed to reach thermal equilibrium for half an hour. The preferred molar volume ratio of oleic acid, octadecene, and cadmium oxide is 15 mmol: 18.8 ml: 20.3 ml. The inert environment is an inert gas protective condition.
[0139] (2) Preparation of TBP-Te solution:
[0140] At room temperature, tellurium powder was dissolved in tributyl phosphate in a glove box and stirred until the solution turned bright yellow. The solution was then removed from the glove box to obtain a TBP-Te solution.
[0141] The preferred molar ratio of cadmium oxide to tellurium powder is 1:1.
[0142] (3) Synthetic cadmium telluride quantum dot ink:
[0143] The TBP-Te solution from step (2) is rapidly injected into the thermal equilibrium solution from step (1). After the injection is complete, the solution is cooled for a long time with an air gun, and then cooled in a water bath. A mixture of toluene and anhydrous ethanol is added to the obtained mixture and centrifuged twice. The centrifuged mixture is then redissolved in a mixture of pyridine and n-propanol to obtain cadmium telluride quantum dot ink. The cadmium telluride quantum dot ink is stable and can be stored in a glove box for a period of time.
[0144] The volume ratio of toluene to anhydrous ethanol is (1-2):(2-4), preferably 1:2;
[0145] The volume ratio of pyridine to n-propanol is (1-2):(2-4), preferably 1:2.
[0146] In some embodiments, the preparation method of the mercury telluride quantum dot ink is as follows:
[0147] (1.1) TOP-Te solution: Te particles are dispersed in tri-n-octylphosphine in an inert environment to form a bright yellow solution, which is called TOP-Te solution; the inert environment is preferably a nitrogen glove box, and the dispersion is preferably stirred; the molar ratio of Te particles to tri-n-octylphosphine is preferably 1:1;
[0148] (1.2) Thermal equilibrium solution: Mercuric chloride is added to oleylamine in an inert environment and heated to 100°C to form a transparent, pale yellow solution; the heating is preferably a heating plate with magnetic stirring function, and the inert environment is preferably a nitrogen glove box; the molar volume ratio of mercuric chloride to oleylamine is 0.1 mmol: 4 mL.
[0149] (1.3) Quenching solution: Mix tri-n-octylphosphine and trichloroethylene and place them in a reaction vessel. Store at low temperature. The volume ratio of tri-n-octylphosphine to trichloroethylene is 0.5 mL: 4 mL. It is preferable to store at low temperature in a refrigerator.
[0150] (1.4) Synthesis of HgTe quantum dot ink using hot injection method: In an inert environment, the thermal equilibrium solution from step (1.2) is brought to thermal equilibrium with the temperature required for the reaction, generally 80℃~100℃. The TOP-Te solution from step (1.1) is then rapidly added, and the reaction time is set, generally 4min~10min. After the reaction is complete, the quenching solution from (1.3) is added to cool the reaction. The ink is then removed from the inert environment and cooled to obtain mercury telluride quantum dot ink. Preferably, the inert environment is a glove box, the cooling is a water bath, the drying is a nitrogen gun, and the centrifugal precipitation is carried out in a centrifuge.
[0151] Generally, the higher the reaction temperature and the longer the reaction time, the larger the quantum dot and the longer the absorption wavelength. Different temperatures and reaction times control the size of the quantum dot, i.e. the cutoff wavelength of absorption, and ultimately achieve a short-wave range of 1.5 to 2.5 μm and a medium-wave range of 3 to 5 μm.
[0152] In some embodiments, the silver telluride quantum dot ink is prepared as follows:
[0153] Silver nitrate was dissolved in oleylamine and oleic acid, and stirred at 70°C for 30 min in a nitrogen glove box to obtain a reaction solution; the preferred molar volume ratio of silver nitrate to oleylamine and oleic acid was 0.2 mmol: 5 mL: 0.5 mL.
[0154] Tellurium particles were dissolved in TOP and heated to 160°C. When the temperature exceeded 140°C, the solution began to turn yellow. The solution was kept at 160°C for 35–45 minutes until it turned into orange TOP-Te. The molar ratio of silver nitrate to tellurium particles was 2:1, and the molar volume ratio of tellurium particles to TOP was 0.1 mmol:0.5 mL.
[0155] When TOP-Te is injected into the reaction solution, the solution immediately turns from orange to black. The reaction time is 10 minutes. After cooling, the solution is stored in a refrigerator.
[0156] A fourth aspect of the present invention is to provide an application of the dual-band quantum dot layer described in the first aspect, or the detector device described in the second aspect, or the detector device prepared by the method described in the third aspect, in visible light (390–760 nm) and infrared light (1.5–5 μm).
[0157] As an optional embodiment of the present invention, the detection device is used in the visible light range of 390–760 nm and the infrared range of 1.5–3 μm, preferably in the range of 1.5–2.5 μm.
[0158] As an optional embodiment of the present invention, the detector is used in visible light (390–760 nm) and infrared light (3–5 μm).
[0159] Numerous specific details are set forth in the following description to provide a thorough understanding of the invention; however, the invention may also be practiced in other ways different from those described herein. Clearly, the embodiments in this specification are only a portion of the embodiments of the invention, and not all of them. The reagents and materials used in these embodiments are of laboratory purity and / or grade, and are not described in detail herein.
[0160] Example 1
[0161] Provides a Figure 2 The fabrication method of the dual-band detector device with the structure shown includes the following steps:
[0162] (1) Preparation of substrate layer: Indium tin oxide with a thickness of 50 nm is magnetron sputtered on the surface of sapphire substrate to form a substrate layer with a thickness of 1 mm.
[0163] (2) Preparation of zinc oxide electron transport layer: 50 μL of ZnO solution is spin-coated onto the surface of the substrate at a spin speed of 3000 r and a spin time of 60 s; then the zinc oxide electron transport layer is annealed on an 80°C hot plate for 10 min to obtain the zinc oxide electron transport layer with a thickness of 10 nm.
[0164] (3) Synthetic cadmium telluride quantum dot ink:
[0165] (3.1) Preparation of thermal equilibrium solution: First, take 1.9g CdO (15mmol) and put it into a three-necked flask, add 18.8ml OA (oleic acid) and 20.3ml ODE (octadecene), put a magnetic ball into the three-necked flask, seal two of the three-necked flasks with a rubber stopper, insert a thermocouple into one end, connect a balloon to the other end with a syringe to prevent it from bursting, and connect the remaining end to a three-way tube. Connect one end of the three-way tube to a vacuum pump and the other end to argon gas.
[0166] First, evacuate the air, then slowly introduce argon gas. Repeat this operation three times to ensure that the three-necked flask is in an argon environment. Then, set the thermocouple to 220°C. After the solution in the three-necked flask is clear, adjust the thermocouple to 270°C and allow it to reach thermal equilibrium for half an hour.
[0167] (3.2) Preparation of TBP-Te solution: At room temperature, dissolve 10g of tellurium powder in 111ml of TBP in a glove box, add magnetic stirring, and wait until the solution turns bright yellow before taking it out of the glove box;
[0168] (3.3) Synthesis of cadmium telluride quantum dot ink: The TBP-Te solution from step (2) is rapidly injected into the thermal equilibrium solution of step (1). After the injection is completed, the three-necked flask is removed from the heating cover and cooled for a long time with an air gun. Then, it is cooled in a water bath. Toluene and anhydrous ethanol (volume ratio, toluene: anhydrous ethanol = 1:2) are added to the obtained mixture. The mixture is centrifuged twice. The centrifuged material is added to a mixture of pyridine and n-propanol (volume ratio, pyridine: n-propanol = 1:2) and redissolved to obtain cadmium telluride quantum dot ink. The cadmium telluride quantum dot ink has a stable shape and can be stored in a glove box for a period of time.
[0169] (4) Preparation of cadmium telluride quantum dot layer:
[0170] The cadmium telluride quantum dot ink was spin-coated onto the surface of the zinc oxide electron transport layer at 800 r-20 s and 1000 r-10 s. The layer was then treated on a hot plate at 60°C for 1 min, followed by treatment in a saturated CdCl2 solution at 60°C for 15 s. Excess CdCl2 solution was then rinsed off with IPA, and finally sintered on a hot plate at 350°C for 20 s. Step (3) was repeated 10 times to obtain a cadmium telluride quantum dot layer with a thickness of 500 nm. The spectral absorption curve of this cadmium telluride quantum dot layer is shown below. Figure 3 As shown;
[0171] (5) Synthetic mercury telluride quantum dot ink:
[0172] (5.1) Synthesis of short-wave infrared quantum dot ink:
[0173] (5.1a) Preparation of thermal equilibrium solution: In a glove box under nitrogen atmosphere, take 27 mg (0.1 mmol) of HgCl2 and place it in a reaction vessel. Add 4 ml of OAM and a magnetic stir bar. Place the reaction vessel on a heating plate and adjust the temperature of the heating plate to 100 °C. Heat for 1 h until a transparent, pale yellow solution is formed. Cool the transparent, pale yellow solution to 80 °C and allow it to reach thermal equilibrium for half an hour.
[0174] (5.1b) Preparation of quenching solution: Take 0.5 ml TOP and 4 ml TCE and place them in a reaction vessel. Mix well and store in a refrigerator.
[0175] (5.1c) Preparation of TOP-Te solution: 0.1 mmol of Te particles were dispersed into 0.1 ml of TOP trioctylphosphine in a nitrogen glove box to form a bright yellow solution;
[0176] (5.1d) Synthesis of mercury telluride quantum dot ink: Take the thermal equilibrium solution from step (5.1a) and rapidly inject it into the TOP-Te solution from step (5.1c) at 80°C. After 15-30 seconds of addition, the solution darkens and turns black. The reaction lasts for 4 minutes. Then, the quenching solution from step (5.1b) is added to cool the reaction. After the reaction is complete, the solution is taken out of the glove box and cooled in a water bath to obtain short-wave infrared quantum dot ink.
[0177] (5.2) Synthesis of mid-wave infrared quantum dot ink:
[0178] (5.2a) Preparation of thermal equilibrium solution: In a glove box under nitrogen atmosphere, take 27 mg (0.1 mmol) of HgCl2 and place it in a reaction vessel. Add 4 ml of OAM and a magnetic stir bar. Place the reaction vessel on a heating plate and adjust the temperature of the heating plate to 105 °C. Heat for 1 h until a transparent, pale yellow solution is formed. Cool the transparent, pale yellow solution to 100 °C and allow it to reach thermal equilibrium for half an hour.
[0179] (5.2b) Preparation of quenching solution: Take 0.5 ml TOP and 4 ml TCE and place them in a reaction vessel. Mix well and store in a refrigerator.
[0180] (5.2c) Preparation of TOP-Te solution: 0.1 mmol of Te particles were dispersed into 0.1 ml of TOP trioctylphosphine in a nitrogen glove box to form a bright yellow solution;
[0181] (5.2d) Synthesis of mercury telluride quantum dot ink: The thermal equilibrium solution from step (5.1a) is rapidly injected into the TOP-Te solution from step (5.1c). After 15-30 seconds, the solution darkens and turns black. The reaction lasts for 10 minutes. Then, the quenching solution from step (5.1b) is added to cool the reaction. After the reaction is complete, the solution is removed from the glove box and cooled in a water bath to obtain the mid-wave infrared quantum dot ink.
[0182] (6) Preparation of mercury telluride quantum dot layers:
[0183] The short-wave infrared quantum dot ink was spin-coated onto the surface of the cadmium telluride quantum dot layer. The spin-coating method was 800r-20s, 1000r-10s. Immediately afterwards, EDT was dropped onto the spin-coated layer for 10s. The residual EDT was rinsed off with IPA, and then HgCl2 solution was dropped onto the layer for 10s. The residual HgCl2 was rinsed off with IPA. Excess IPA was removed using a spin coater. Step (4) was repeated 10 times to obtain the intrinsic layer of mercury telluride quantum dots. The spectral absorption curve of the intrinsic layer of mercury telluride quantum dots is shown below. Figure 4 As shown;
[0184] (7) Synthetic silver telluride quantum dot ink:
[0185] Silver nitrate (34 mg, 0.2 mmol) was dissolved in oleylamine (5 mL) and oleic acid (0.5 mL) and stirred at 70 °C for 30 min in a nitrogen glove box.
[0186] Dissolve tellurium particles in TOP (0.5 mL) and rapidly heat the clear solution to 160 °C. The solution begins to turn yellow when the temperature exceeds 140 °C and is maintained at 160 °C for 35–45 min until it turns into orange TOP-Te.
[0187] TOP-Te (0.1 mL, 0.1 mmol) was injected into the reaction solution. The solution immediately turned from orange to black, and the reaction time was 10 min. The reaction mixture was then cooled and stored in a refrigerator.
[0188] (8) Preparation of silver telluride quantum dot doped layer:
[0189] The silver telluride quantum dot ink was spin-coated onto the intrinsic layer of the mercury telluride quantum dot at 3000 r for 60 s. Then, HgCl2 solution was added dropwise for 10 s. The residual HgCl2 was rinsed off with IPA to prepare the silver telluride quantum dot doped layer.
[0190] (9) Preparation of the top electrode layer:
[0191] A 40 nm thick layer of gold is deposited on the surface of the silver telluride quantum dot doped layer.
[0192] This embodiment fabricated a visible-infrared fusion detection device and performed finite element simulation analysis using COMSOL software. Figure 5 , Figure 6 , Figure 5 The diagram shows the band structure of the detection device, where the band gap of mercury telluride quantum dots is 0.52 eV and the band gap of cadmium telluride quantum dots is 1.36 eV. Figure 6 The spectral response of the detection device shows that there is a peak in the visible light region and a peak in the short-wave infrared region, thus realizing a dual-band fusion response.
[0193] Example 2
[0194] A method for fabricating a dual-band focal plane array device is provided: it includes,
[0195] (1) Select a focal plane array and arrange readout circuits on the surface of the focal plane array;
[0196] (2) The quantum dot ink is coated on the surface of the readout circuit according to the description in Example 1, and then the device is packaged to obtain a dual-band focal plane array device.
[0197] The dual-band focal plane array device is mounted in a housing, and the readout circuit is led to the pins of the housing by wires. These pins are then connected to other devices through wires on the printed circuit board, thereby realizing the connection between the internal chip and the external circuit.
[0198] Comparative Example 1
[0199] A detector device prepared for Chinese invention patent application (application number: 2022107534911, application date: 2022-06-30).
[0200] Compared to Comparative Example 1, the detection device designed in this invention can simultaneously detect infrared and visible light under the same bias voltage.
[0201] The detector operates at room temperature, has a pixel responsivity of 0.6 A / W, and a pixel detectivity of 1 × 10⁻⁶. 11 Jones, with a power conversion efficiency of 15%. The pixel responsivity, pixel detectivity, and power conversion efficiency are all calculated according to the formulas specified in the People's Republic of China National Standard GB / T17444-1998 "Technical Specification for Testing Characteristic Parameters of Infrared Focal Plane Arrays". Therefore, the detector device designed in this invention has high photoelectric conversion efficiency and good detection efficiency.
[0202] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0203] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments described herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A dual-band quantum dot layer, characterized in that, The quantum dot layer comprises an infrared photosensitive film layer and a visible light photosensitive film layer combined together, and the infrared photosensitive film layer and the visible light photosensitive film layer form two co-directional PN heterojunctions; The infrared photosensitive film layer is composed of a chalcogenide silver quantum dot doping layer and a chalcogenide mercury quantum dot intrinsic layer, and the chalcogenide silver quantum dot doping layer and the chalcogenide mercury quantum dot intrinsic layer form a PN heterojunction. The visible light photosensitive film layer is composed of a zinc oxide electron transport layer and a cadmium telluride quantum dot layer, and the cadmium telluride quantum dot layer and the zinc oxide electron transport layer form the remaining PN heterojunction.
2. The quantum dot layer according to claim 1, characterized in that, The thickness of the chalcogenide silver quantum dot doped layer is less than the thickness of the chalcogenide mercury quantum dot intrinsic layer.
3. The quantum dot layer according to claim 1, characterized in that, The material of the chalcogenide silver quantum dot doped layer is any one of silver sulfide, silver selenide, and silver telluride.
4. The quantum dot layer according to claim 3, characterized in that, The material of the chalcogenide silver quantum dot doped layer is silver telluride.
5. The quantum dot layer according to claim 1, characterized in that, The intrinsic material of the chalcogenide mercury quantum dot layer is any one of mercury sulfide, mercury selenide, or mercury telluride.
6. The quantum dot layer according to claim 5, characterized in that, The intrinsic layer of the chalcogenide mercury quantum dots is made of mercury telluride.
7. The quantum dot layer according to claim 1, characterized in that, The thickness of the zinc oxide electron transport layer is less than the thickness of the cadmium telluride quantum dot layer.
8. A detection device, characterized in that, The detector includes at least one pixel, the pixel comprising: a substrate layer, at least one dual-band quantum dot layer as described in any one of claims 1 to 7, and a top electrode layer arranged sequentially from top to bottom.
9. The detector according to claim 8, characterized in that, The detector includes a plurality of pixels, which are arranged in a row and column array.
10. A method for manufacturing the detector device according to claim 8 or 9, characterized in that, The preparation method includes sequentially laminating a visible light photosensitive film layer, an infrared photosensitive film layer, and a top electrode layer on the surface of a substrate layer, wherein the infrared photosensitive film layer and the visible light photosensitive film layer constitute two co-directional PN heterojunctions.
11. The application of a dual-band quantum dot layer according to any one of claims 1 to 7, or a detector according to claim 8 or 9, or a detector prepared by the method according to claim 10, in visible light (390 to 760 nm) and infrared (1.5 to 5 μm).
Citation Information
Patent Citations
Imaging device, preparation method thereof, imaging array and preparation method thereof
CN114551486A
Non-inverted bonding body type dual-band quantum dot pixel, focal plane array and preparation method and application of non-inverted bonding body type dual-band quantum dot pixel and focal plane array