A comprehensive utilization method of high-arsenic antimony gold slag
By using alkaline thermal method, sodium sulfide and oxidative acid leaching method to separate arsenic, antimony and copper in gold slag under normal pressure, the problems of separation difficulty and environmental pollution in the existing technology are solved, and efficient and economical metal synthesis is achieved. use.
Patent Information
- Application Number
- CN202110898655.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-08-05
AI Technical Summary
It is difficult for the existing technology to efficiently separate arsenic, antimony and copper from high-arsenic antimony gold slag under normal pressure, and the traditional pyrotechnic process consumes high energy and is not environmentally friendly, resulting in environmental pollution.
The alkali thermal method is used to separate arsenic under normal pressure, sodium sulfide is used to separate antimony, and copper is separated through oxidative acid leaching. Finally, a gold extracting agent is used to extract gold, achieving cascade comprehensive utilization of metal elements.
It achieves efficient separation of arsenic, antimony and copper under normal pressure, reduces equipment requirements and operational difficulty, is suitable for industrial processes, and significantly improves gold extraction efficiency and economic benefits.
Smart Images

Figure CN115704060B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a comprehensive utilization method of high-arsenic antimony-gold slag. Background Art
[0002] In recent years, with the advancement of high-temperature chlorination metallurgy technology, chlorination volatilization technology has been increasingly adopted by domestic gold companies. Usually, chlorination volatilization uses cyanide tailings and calcium chloride as the main raw materials, and reacts in a high-temperature furnace after pelletizing. The high-temperature flue gas produced by volatilization is sprayed and washed to generate slurry. The slurry is separated into solid and liquid. The filtrate after separation is replaced by iron powder to produce replacement slag containing 100-400g / t of gold and 15-20% of copper. The gold grade in the slag is low and it is difficult to be used directly for refining.
[0003] In addition to gold, this type of slag usually contains valuable metal elements such as silver, copper and antimony, which have extremely high utilization value. In addition, arsenic is also an important substance contained in the slag. Arsenic is a highly toxic carcinogen. Improper disposal will cause great harm to the ecological environment. Arsenic pollution has become a global problem. Therefore, while this type of gold slag is being utilized as a resource, the environmental problems it causes cannot be ignored.
[0004] Arsenic and antimony coexist in this type of slag, and arsenic and antimony have similar chemical properties, so it is very difficult to separate the two. Although the separation of arsenic and antimony can be achieved by volatilizing arsenic and antimony in steps by utilizing the difference in the volatilization temperature of arsenic and antimony oxides, the pyrometallurgical process has high energy consumption, the separation of arsenic and antimony is not thorough, and the arsenic-containing dust produced is prone to secondary environmental pollution. Relatively speaking, the hydrometallurgical method is cleaner and more environmentally friendly. Pressurized oxidation is a commonly used method. Under pressurized oxidation conditions, arsenic can be leached into the solution, while antimony is retained in the slag in the form of NaSb(OH)6. However, the cost of pressurized equipment is high, and the process operation requirements are harsh, which is not conducive to production. In view of the unfavorable factors of pyrometallurgy and pressurized processes, the separation of arsenic and antimony under normal pressure has received widespread attention. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a comprehensive utilization method of high-arsenic antimony gold slag, which can efficiently remove arsenic, antimony and copper from the gold slag, thereby realizing the cascade comprehensive utilization of arsenic, antimony, copper and gold.
[0006] The present invention provides a comprehensive utilization method of high-arsenic antimony gold slag, comprising the following steps:
[0007] Step S1: mixing the finely ground gold slag with an alkaline solution, and after sufficient reaction, separating the solid and the liquid, evaporating and concentrating the filtrate to obtain an arsenate crystal product, and the crystallization mother liquor is further used to react with the finely ground gold slag;
[0008] Step S2: the filter residue obtained in step S1 is adjusted to pH 8-12, sodium sulfide is added to react, solid-liquid separation is performed after the reaction, the filtrate is evaporated, concentrated and crystallized to obtain an antimony salt product, and the crystallization mother liquor is further used to react with the filter residue obtained in step S1;
[0009] Step S3: mixing the filter residue obtained in step S2 with an acid, and adding an oxidant to carry out an oxidative acid leaching reaction, and separating the solid and liquid after the reaction to obtain a copper-containing filtrate and a copper-removed slag;
[0010] Step S4: extracting the copper-containing filtrate to prepare a copper sulfate solution; treating the copper-removing slag with a gold extracting agent to extract gold therein.
[0011] Preferably, in step S1, the particle size of the gold slag after fine grinding is less than 0.075 mm.
[0012] Preferably, in step S1, the reaction temperature is 50-90°C.
[0013] Preferably, in step S2, the reaction temperature is 50-80°C.
[0014] Preferably, in step S1, the alkaline solution is one or more of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution and ammonia water.
[0015] Preferably, the concentration of the alkaline solution is 0.5-5 mol / L, and the solid-to-liquid ratio of the finely ground gold slag to the alkaline solution is 1:2-9.
[0016] Preferably, in step S2, the concentration of sodium sulfide is 0.5-4 mol / L, and after adding sodium sulfide, the solid-liquid ratio in the solution is 1:2-9.
[0017] Preferably, in step S3, the acid is one or more of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, acetic acid and hydrofluoric acid, the mass concentration of the acid is 5-50%, and the solid-liquid ratio in the reaction solution is 1:2-7.
[0018] Preferably, in step S3, the oxidant is hydrogen peroxide, ozone, trivalent iron salt, manganese dioxide, potassium permanganate or chlorate.
[0019] Preferably, in step S3, the amount of the oxidant used is 0.5 to 2 times the molar content of copper in the filter residue obtained in step S2.
[0020] Compared with the prior art, the comprehensive utilization method of high-arsenic antimony-gold slag of the present invention is
[0021] The process first uses an alkali-thermal method to separate and extract arsenic from gold mud, then uses sodium sulfide to leach antimony, and then separates copper and other substances through oxidative acid leaching. Finally, the enriched gold slag is extracted using a gold extracting agent. The main characteristics of this process are that arsenic is separated by an alkali-thermal method under normal pressure, which can reduce the arsenic content to less than 0.5%; antimony is separated by sodium sulfide under alkaline conditions, and the antimony content is reduced to less than 0.5%; copper and other substances are separated under oxidative acid leaching conditions, and the copper content is reduced to less than 0.3%, and finally gold-rich slag is obtained. The whole process of the present invention adopts a hydrometallurgical method, and arsenic, antimony, copper and other substances in the gold mud are extracted in stages by a selective separation method, so as to realize the clean and high-value comprehensive utilization of the slag.
[0022] The present invention gradually separates a variety of metal elements under normal pressure conditions, reduces the requirements for equipment, is easy to operate, is suitable for industrial processes, and has outstanding economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic flow chart showing a method for selectively separating high-arsenic antimony-gold slag according to a specific embodiment of the present invention. DETAILED DESCRIPTION
[0024] In order to further understand the present invention, the embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the present invention.
[0025] The embodiment of the present invention discloses a comprehensive utilization method of high-arsenic antimony gold slag, comprising the following steps:
[0026] Step S1: mixing the finely ground gold slag with an alkaline solution, and after sufficient reaction, separating the solid and the liquid, evaporating and concentrating the filtrate to obtain an arsenate crystal product, and the crystallization mother liquor is further used to react with the finely ground gold slag;
[0027] Step S2: the filter residue obtained in step S1 is adjusted to pH 8-12, sodium sulfide is added to react, solid-liquid separation is performed after the reaction, the filtrate is evaporated, concentrated and crystallized to obtain an antimony salt product, and the crystallization mother liquor is further used to react with the filter residue obtained in step S1;
[0028] Step S3: mixing the filter residue obtained in step S2 with an acid, and adding an oxidant to carry out an oxidative acid leaching reaction, and separating the solid and liquid after the reaction to obtain a copper-containing filtrate and a copper-removed slag;
[0029] Step S4: extracting the copper-containing filtrate to prepare a copper sulfate solution; treating the copper-removing slag with a gold extracting agent to extract gold therein.
[0030] The present invention processes the gold slag produced by the chlorination volatilization technology. The gold grade in the gold slag is relatively low. After being processed by the method of the present invention, arsenic, antimony, copper and other substances can be selectively separated, and gold enrichment and efficient recovery are finally achieved. Generally, gold can be enriched more than twice, and after removing impurities such as arsenic and antimony that interfere with gold extraction, the gold extraction efficiency can be significantly improved and the reagent consumption can be reduced.
[0031] The following combination Figure 1 The steps of the method of the present invention are described in detail:
[0032] Step S1: mixing the finely ground gold slag with an alkaline solution, and after sufficient reaction, separating the solid and the liquid, evaporating and concentrating the filtrate to obtain an arsenate crystal product, and the crystallization mother liquor is further used to react with the finely ground gold slag.
[0033] This step is to separate and extract arsenic from gold slag using an alkali-thermal method.
[0034] In order to allow the gold slag to fully react with the alkaline solution, it is preferred to finely grind the gold slag before reacting.
[0035] Preferably, the particle size of the gold slag after fine grinding is less than 0.075 mm.
[0036] The alkaline solution is preferably one or more of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution and ammonia water; more preferably sodium hydroxide solution.
[0037] The concentration of the alkaline solution is preferably 0.5-5 mol / L, more preferably 2-4 mol / L; the solid-liquid ratio of the finely ground gold slag to the alkaline solution is preferably 1:2-9, more preferably 1:3-5.
[0038] In the step S1, the reaction temperature is preferably 50 to 90°C, more preferably 60 to 80°C.
[0039] After sufficient reaction, solid-liquid separation can be selected by filtration separation. Filtrate and filter residue are separated. The filtrate is evaporated, concentrated and crystallized to obtain arsenate crystals. The crystallization mother liquor can be recycled and used for the next reaction with finely ground gold residue.
[0040] Step S2: The filter residue obtained in step S1 is adjusted to pH 8-12, sodium sulfide is added to react, solid-liquid separation is performed after the reaction, and the filtrate is evaporated, concentrated and crystallized to obtain an antimony salt product, and the crystallization mother liquor is further used to react with the filter residue obtained in step S1.
[0041] This step is used to separate antimony.
[0042] The pH value of the filter residue obtained in step S1 is adjusted to 8-12. The adjustment method is preferably: adding an alkaline solution to the filter residue obtained in step S1 to adjust the pH value. The alkaline solution is preferably one or more of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution and ammonia water, and more preferably sodium hydroxide solution.
[0043] The concentration of the sodium sulfide is preferably 0.5-4 mol / L. After the sodium sulfide is added, the solid-liquid ratio in the solution is 1:2-9.
[0044] In the step S2, the reaction temperature is preferably 50-80°C.
[0045] Under the above conditions, antimony can be leached into the solution, and the antimony content in the leached slag can be controlled to be below 0.5%.
[0046] After the reaction, the solid and liquid are separated and filtered to obtain a filtrate and a filter residue. The filtrate is evaporated, concentrated and crystallized to obtain an antimony salt product, and the crystallization mother liquor can be recycled and used for the next reaction with the filter residue obtained in step S1.
[0047] Step S3: The filter residue obtained in step S2 is mixed with an acid, and an oxidant is added to carry out an oxidative acid leaching reaction, and after the reaction, solid-liquid separation is performed to obtain a copper-containing filtrate and a copper-removed slag.
[0048] In this step, copper is separated by oxidative acid leaching, and the copper-removed slag is the enriched gold slag, and the copper-removed slag is extracted by a gold extracting agent.
[0049] The acid is preferably one or more of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, acetic acid and hydrofluoric acid, more preferably sulfuric acid; the mass concentration of the acid is preferably 5-50%, and the solid-liquid ratio in the reaction solution is preferably 1:2-7.
[0050] The oxidant is preferably hydrogen peroxide, ozone, ferric iron, manganese dioxide, potassium permanganate or chlorate, and more preferably hydrogen peroxide. The amount of the oxidant is 0.5 to 2 times the molar content of copper in the filter residue obtained in step S2.
[0051] Under the above conditions, copper can be leached into the solution by stirring and leaching, and the copper content in the slag can be controlled to below 0.3%.
[0052] After the reaction, the solid-liquid separation can be carried out by filtering to obtain a copper-containing filtrate and copper-removed slag.
[0053] Step S4: extracting the copper-containing filtrate to prepare a copper sulfate solution; treating the copper-removing slag with a gold extracting agent to extract gold therein.
[0054] The copper is extracted by solvent extraction to prepare copper sulfate solution, and the raffinate is returned to the system for recycling.
[0055] After the extraction of arsenic, antimony and copper, the gold in the slag is further extracted using a gold extracting agent.
[0056] The present invention adopts a fully hydrometallurgical process, which can efficiently remove arsenic, antimony and copper from gold slag. The contents of arsenic, antimony and copper in the slag after leaching are respectively reduced to below 0.5%, 0.5% and 0.3%, thereby realizing the cascade comprehensive utilization of arsenic, antimony, copper and gold.
[0057] The whole process of the present invention is carried out under normal pressure, the requirements for equipment are greatly reduced, the operation is easy, the invention is suitable for industrial processes, and the economic benefits are more outstanding.
[0058] In order to further understand the present invention, the comprehensive utilization method of high-arsenic antimony gold slag provided by the present invention is described in detail below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0059] Example 1
[0060] The raw material used in this embodiment is fresh arsenic-antimony-gold slag obtained from a certain enterprise. The moisture content in the slag is high. After drying, the contents of the main components in the slag are: As 10.7%; Sb 22.62%; Cu 16.7; Au 300g / t.
[0061] The gold slag was finely ground to less than 0.075 mm, 30 g of the gold slag was put into a stirring tank, 150 ml of a 2 mol / L sodium hydroxide solution was added, and the mixture was heated to 80°C and stirred for 6 hours. The mixture was filtered and separated, and the leaching solution was evaporated, concentrated and crystallized to prepare sodium arsenate. The arsenic content in the filter residue was 0.3%, the antimony content was 24.5%, and the copper content was 20.5%.
[0062] 30g of arsenic removal residue was placed in a stirring tank, 200ml of water was added and stirred, the pH was adjusted to 12 with NaOH, 40g of sodium sulfide was added, and the mixture was heated to 60°C and stirred for 5 hours. After filtration and separation, the filtrate was evaporated and crystallized; the arsenic content in the residue was 0.2%, the antimony content was 0.3%, and the copper content was 28.3%.
[0063] Take 30g of antimony-free slag and put it into a stirring tank, add 150ml of 30% sulfuric acid solution, add 5g of manganese dioxide, heat to 80℃, stir for 6 hours and filter. The arsenic content in the filter residue is 0.3%, the antimony content is 0.5%, the copper content is 0.1%, and the gold content is 800g / t. Extract the copper-containing filtrate to prepare copper sulfate solution.
[0064] Example 2
[0065] The raw material used in this embodiment is arsenic-antimony-gold slag obtained from a certain enterprise. The slag has dried and agglomerated after long-term storage. After drying and sampling, the contents of the main components in the slag are: As 6.8%; Sb 13.4%; Cu 21.8; Au 180g / t.
[0066] The gold slag was finely ground to less than 0.075 mm, 30 g of the gold slag was put into a stirring tank, 100 ml of 2 mol / L sodium hydroxide was added, and the mixture was heated to 60°C and stirred for 4 hours. The mixture was filtered and separated, and the leaching solution was evaporated, concentrated and crystallized to prepare sodium arsenate. The arsenic content in the filter residue was 0.2%, the antimony content was 16.5%, and the copper content was 25.5%.
[0067] 30g of arsenic removal residue was placed in a stirring tank, 120ml of water was added and stirred, the pH was adjusted to 10 with NaOH, 30g of sodium sulfide was added, and the mixture was heated to 70°C and stirred for 5 hours. After filtration and separation, the filtrate was evaporated and crystallized; the arsenic content in the residue was 0.2%, the antimony content was 0.4%, and the copper content was 33.2%.
[0068] Take 30g of antimony-free slag and put it into a stirring tank, add 200ml of 25% sulfuric acid solution, add 10ml of hydrogen peroxide, heat to 60℃, stir for 5 hours and filter. The arsenic content in the filter residue is 0.2%, the antimony content is 0.5%, the copper content is 0.2%, and the gold content is 548g / t.
[0069] Example 3
[0070] The raw material used in this embodiment is arsenic-antimony-gold slag obtained from a certain enterprise. The slag still contains a certain amount of moisture after being placed for a period of time. After drying and sampling, the contents of the main components in the slag are: As 15.6%; Sb 8.6%; Cu 16.8; Au 264g / t.
[0071] The gold slag was finely ground to less than 0.075 mm, 30 g of the gold slag was put into a stirring tank, 120 ml of a 2.5 mol / L sodium hydroxide solution was added, and the mixture was heated to 85°C and stirred for 5 hours. The mixture was filtered and separated, and the leaching solution was evaporated, concentrated and crystallized to prepare sodium arsenate. The arsenic content in the filter residue was 0.1%, the antimony content was 10.5%, and the copper content was 18.9%.
[0072] Take 30g of arsenic removal residue and put it into a stirring tank, add 100ml of water and stir, adjust the pH to 12 with NaOH, add 25g of sodium sulfide, heat to 60℃ and stir for 5 hours. After filtration and separation, the filtrate is evaporated and crystallized; the arsenic content in the residue is less than 0.1%, the antimony content is 0.3%, and the copper content is 25.8%.
[0073] Take 30g of antimony-free slag and put it into a stirring tank, add 150ml of 20% sulfuric acid solution, add 5g of potassium permanganate, heat to 70℃, stir for 8 hours and filter. The arsenic content in the filter residue is 0.1%, the antimony content is 0.3%, the copper content is 0.3%, and the gold content is 680g / t.
[0074] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0075] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A comprehensive utilization method of high-arsenic antimony-gold slag, characterized in that: The following steps are involved: Step S1: mixing the finely ground gold slag with an alkaline solution, and after sufficient reaction, separating the solid and the liquid, evaporating and concentrating the filtrate to obtain an arsenate crystal product, and the crystallization mother liquor is further used to react with the finely ground gold slag; Step S2: the filter residue obtained in step S1 is adjusted to pH 8-12, sodium sulfide is added to react, solid-liquid separation is performed after the reaction, the filtrate is evaporated, concentrated and crystallized to obtain an antimony salt product, and the crystallization mother liquor is further used to react with the filter residue obtained in step S1; Step S3: mixing the filter residue obtained in step S2 with an acid, and adding an oxidant to carry out an oxidative acid leaching reaction, and separating the solid and liquid after the reaction to obtain a copper-containing filtrate and a copper-removed slag; Step S4: extracting the copper-containing filtrate to prepare a copper sulfate solution; treating the copper-removing slag with a gold extracting agent to extract gold therein.
2. The comprehensive utilization method of high-arsenic antimony gold slag according to claim 1 is characterized in that: In the step S1, the particle size of the gold slag after fine grinding is less than 0.075 mm.
3. The comprehensive utilization method of high-arsenic antimony gold slag according to claim 2 is characterized in that: In the step S1, the reaction temperature is 50-90°C.
4. The comprehensive utilization method of high-arsenic antimony-gold slag according to claim 1 is characterized in that: In the step S2, the reaction temperature is 50-80°C.
5. The comprehensive utilization method of high-arsenic antimony-gold slag according to claim 1 is characterized in that: In step S1, the alkaline solution is one or more of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution and ammonia water.
6. The comprehensive utilization method of high-arsenic antimony-gold slag according to claim 5 is characterized in that: The concentration of the alkaline solution is 0.5-5 mol / L, and the solid-liquid ratio of the finely ground gold slag to the alkaline solution is 1:2-9.
7. The comprehensive utilization method of high-arsenic antimony-gold slag according to claim 1 is characterized in that: In the step S2, the concentration of the sodium sulfide is 0.5-4 mol / L, and after the sodium sulfide is added, the solid-liquid ratio in the solution is 1:2-9.
8. The comprehensive utilization method of high-arsenic antimony-gold slag according to claim 1 is characterized in that: In step S3, the acid is one or more of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, acetic acid and hydrofluoric acid, the mass concentration of the acid is 5-50%, and the solid-liquid ratio in the reaction solution is 1:2-7.
9. The comprehensive utilization method of high-arsenic antimony-gold slag according to claim 1, characterized in that: In step S3, the oxidant is hydrogen peroxide, ozone, trivalent iron salt, manganese dioxide, potassium permanganate or chlorate.
10. The comprehensive utilization method of high-arsenic antimony-gold slag according to claim 1, characterized in that: In step S3, the amount of the oxidant used is 0.5 to 2 times the molar content of copper in the filter residue obtained in step S2.
Citation Information
Patent Citations
Method for recovering copper through copper anode mud supersonic pretreatment
CN103320616A
Method for efficiently cleaning and removing arsenic in copper-containing slag
CN107099669A
Method for separating copper and arsenic from copper-arsenic slag
CN107475519A
Method for recovering alkali, selenium and arsenic in arsenic-alkali residue from antimony smelting
CN110143604A
Method for recovering valuable metals after alkaline leaching and dehalogenation of circuit board smelting smoke dust
CN112063850A