Defective Ni-MOFs desulfurization adsorbent and preparation method and application thereof
The defective Ni-MOFs adsorbent was prepared by solvothermal method, which solved the problem of low adsorption capacity and low adsorption rate, achieved excellent adsorption performance for thiophene sulfides, and was suitable for the efficient removal of sulfides in oil.
Patent Information
- Application Number
- CN202211260862.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-14
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-10-14
AI Technical Summary
The existing adsorption desulfurization agents have low adsorption capacity and adsorption rate, and the metal organic framework has good desulfurization effect but is difficult to form. The desulfurization ability of molecular sieves is limited, making it difficult to effectively increase the sulfur capacity of MOFs in adsorption desulfurization.
The defective Ni-MOFs desulfurization adsorbent was prepared using a solvothermal method. The template agent N,N-dimethyloctadecylamine was added to the nickel source and 2,5-dihydroxyterephthalic acid precursor solution. After the template agent was removed, Obtain a uniformly distributed mesoporous structure, expand the mesopore diameter to 2-5nm, increase unsaturated nickel active sites, and improve the adsorption performance of sulfide.
The adsorption performance of defective Ni-MOFs for thiophene sulfides is significantly improved, the interaction with sulfides is enhanced, the adsorption capacity and stability are improved, and it is suitable for the adsorption and removal of sulfides in oil products.
Smart Images

Figure CN115739039B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorption desulfurization, and specifically relates to a defective Ni-MOFs desulfurization adsorbent and a preparation method and application thereof. Background Art
[0002] With the rapid development of the world economy, the demand for energy in social industrial production is increasing rapidly. Under the background of energy shortage, people have developed a variety of energy-generating methods, such as wind energy, hydropower, bioenergy and other new energy sources. However, it is worth noting that the fossil energy dominated by coal and oil is still the most used in the world energy system. With the extensive use of fossil energy, environmental problems have also followed. The organic sulfur compounds in fossil fuels produce pollutants such as SO2 after combustion, which will cause great damage to the environment, such as acid rain, haze, etc., and even produce carcinogenic effects after being inhaled by the human body. In addition, sulfur-containing substances have irreversible corrosion damage and catalyst poisoning effects on production equipment and exhaust gas treatment systems in transportation vehicles. How to effectively and reasonably control the sulfur content in fossil fuels is a major problem that every country urgently needs to solve.
[0003] The desulfurization technologies widely used in the world include hydrodesulfurization (HDS), oxidative desulfurization (ODS), adsorptive desulfurization (ADS), biological desulfurization (BDS) and extractive desulfurization (EDS).
[0004] Hydrodesulfurization (HDS) is the main method for producing clean fuel oil. In the actual production process, hydrodesulfurization has the advantages of high efficiency and low cost. However, when aromatic sulfur compounds (such as thiophene and benzothiophene) coexist with olefins, excessive hydrogenation leads to serious loss of octane number, making it difficult to produce ultra-low sulfur or even sulfur-free fuel. In addition, the traditional hydrodesulfurization catalyst preparation method has problems such as strong interaction between active metal and carrier, low degree of sulfurization, long start-up cycle and environmental unfriendliness. Therefore, non-hydrodesulfurization technology has gradually become a research hotspot.
[0005] Adsorption desulfurization (ADS) is an important alternative process to hydrodesulfurization, which uses porous materials or metal sites loaded on inorganic carriers to achieve the purpose of desulfurization through physical or chemical adsorption. It has the advantages of low investment, low energy consumption, high removal accuracy, simple process flow, mild operating conditions and high desulfurization efficiency. Compared with HDS, it will not reduce the octane number of oil products. This technology has gradually become a hot research direction for desulfurization.
[0006] The selection of adsorbent is a complex issue. The adsorbent used for fuel desulfurization should have the advantages of large adsorption capacity, fast adsorption rate, large separation factor, high stability, etc. At the same time, the regeneration performance of the adsorbent should also be considered. Many porous materials have been used as desulfurization adsorbents, such as activated carbon, molecular sieves, metal oxides and metal organic framework materials.
[0007] Chinese patent CN106861649A discloses an oil desulfurization adsorbent based on metal-organic framework compounds and its preparation method. MOFs and γ-Al2O3 are compounded together by hydrothermal method to obtain a supported composite material MOFs@Al2O3. The adsorption and removal of dibenzothiophene by this material reaches 82.3mg S / g MOF. Chinese patent CN114733487A discloses a bimetallic Cu / Zr-MOFs adsorption desulfurizer and its preparation method and application. The internal extension growth method is used to make small crystal MOF-808 organically embedded on the surface of MOF-199 (Cu), and the bimetallic adsorption desulfurizer Cu / Zr-MOFs with an open core-satellite structure is prepared. It has good adsorption and desulfurization performance, and the adsorption sulfur capacity can reach up to 56mg S / g.
[0008] In summary, although some preparation methods of adsorbents for oil desulfurization have been reported in previous literature, the existing adsorbents have the following problems: a. The pore volume and specific surface area of the adsorbent are low, and the adsorption sulfur capacity is limited; b. The metal organic framework has a good desulfurization effect, but it is difficult to form and inconvenient to use; c. The desulfurization capacity of the molecular sieve adsorbent is limited. Therefore, further exploration is needed to improve the sulfur capacity of MOFs in adsorption desulfurization. Summary of the invention
[0009] The present invention aims to solve the problems of low adsorption capacity and low adsorption rate of molecular sieve fuel desulfurization adsorbent at least to a certain extent. To this end, one purpose of the present invention is to propose a defective Ni-MOFs desulfurization adsorbent and its preparation method and application. The defective Ni-MOFs desulfurization adsorbent prepared by the method retains a certain proportion of the original micropores while its mesopore diameter can be expanded to 2-5nm, and has good stability. While removing the template agent, the unsaturated metal sites of the nickel core are increased, and a uniform mesopore distribution is introduced into the original microporous material, which promotes more unsaturated nickel active sites to be fully exposed. The large pore size is conducive to the mass transfer process. The exposed unsaturated nickel active sites enhance the interaction with sulfides and greatly increase the adsorption amount. These two advantages make the defective Ni-MOFs have excellent adsorption performance for sulfides.
[0010] In one aspect of the present invention, the present invention provides a method for preparing a defective Ni-MOFs desulfurization adsorbent. According to an embodiment of the present invention, the method comprises the following steps:
[0011] (1) dissolving 2,5-dihydroxyterephthalic acid and N,N-dimethyloctadecylamine in tetrahydrofuran to obtain a solution A;
[0012] (2) dissolving the nickel source compound in deionized water to obtain solution B;
[0013] (3) The solution A and the solution B are mixed evenly, loaded into a reaction kettle lined with polytetrafluoroethylene, placed in an oven for constant temperature crystallization, cooled to room temperature, centrifuged, washed and dried to obtain a defective Ni-MOFs desulfurization adsorbent.
[0014] According to the method for preparing a defective Ni-MOFs desulfurization adsorbent according to an embodiment of the present invention, a template agent N,N-dimethyloctadecylamine is added to a precursor solution with a nickel source and 2,5-dihydroxyterephthalic acid as raw materials, and a defective Ni-MOFs desulfurization adsorbent is prepared by a solvothermal method. After the template agent N,N-dimethyloctadecylamine is removed, uniformly distributed mesopores can be obtained. The defective Ni-MOFs desulfurization adsorbent prepared by this method retains a certain proportion of the original micropores, and its mesopore diameter can be expanded to 2-5nm, and has good stability. While removing the template agent, the unsaturated metal sites of the nickel core are increased, and a uniform mesopore distribution is introduced into the original microporous material, which promotes more unsaturated nickel active sites to be fully exposed. The large pore size is conducive to the mass transfer process, and the exposed unsaturated nickel active sites enhance the interaction with the sulfide, greatly improving the adsorption amount. These two advantages make defective Ni-MOFs have excellent adsorption properties for thiophene sulfides.
[0015] In addition, the method for preparing a defective Ni-MOFs desulfurization adsorbent according to the above embodiment of the present invention may also have the following additional technical features:
[0016] In some embodiments of the present invention, the mass volume ratio of the 2,5-dihydroxyterephthalic acid, the N,N-dimethyloctadecylamine, the nickel source compound, the tetrahydrofuran and the deionized water is (0.1-0.2) g: (0.20-0.28) g: (0.2-0.4) g: (10-30) mL: (10-30) mL.
[0017] In some embodiments of the present invention, in step (2), the nickel source compound includes at least one of nickel nitrate hexahydrate, nickel acetate tetrahydrate, nickel sulfate hexahydrate and nickel chloride hexahydrate.
[0018] In some embodiments of the present invention, in step (3), the crystallization temperature is 90-120° C. and the time is 48-96 hours.
[0019] In some embodiments of the present invention, in step (3), the drying temperature is 80-100° C. and the drying time is 8-12 hours.
[0020] In some embodiments of the present invention, in step (3), the washing comprises: first washing with deionized water and then washing with ethanol.
[0021] In the second aspect of the present invention, the present invention proposes a defective Ni-MOFs desulfurization adsorbent. According to an embodiment of the present invention, the defective Ni-MOFs desulfurization adsorbent is prepared by the above method. As a result, the defective Ni-MOFs desulfurization adsorbent has a uniform mesopore distribution and more unsaturated active sites, wherein the large pore size is conducive to the mass transfer process, and the exposed unsaturated nickel active sites enhance the interaction with the sulfide, greatly improving the adsorption amount. These two advantages make the defective Ni-MOFs desulfurization adsorbent have excellent adsorption performance for sulfides in oil products.
[0022] In the third aspect of the present invention, the present invention proposes an application of a defective Ni-MOFs desulfurization adsorbent. According to an embodiment of the present invention, the defective Ni-MOFs desulfurization adsorbent is prepared by the above method, and the application includes the application of adsorption and removal of sulfides in oil products.
[0023] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0025] Figure 1 It is a process flow chart of a method for preparing a defective Ni-MOFs desulfurization adsorbent according to an embodiment of the present invention. DETAILED DESCRIPTION
[0026] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0027] In one aspect of the present invention, the present invention provides a method for preparing a defective Ni-MOFs desulfurization adsorbent. According to an embodiment of the present invention, reference Figure 1 , the method comprises the following steps:
[0028] S100: Dissolve 2,5-dihydroxyterephthalic acid and N,N-dimethyloctadecylamine in tetrahydrofuran
[0029] In this step, 2,5-dihydroxyterephthalic acid and N,N-dimethyloctadecylamine are dissolved in tetrahydrofuran to obtain solution A. Specifically, the mass volume ratio of 2,5-dihydroxyterephthalic acid, N,N-dimethyloctadecylamine and tetrahydrofuran is (0.10-0.20) g: (0.20-0.28) g: (10-30) mL. The inventors have found that when the ratio of each component is too high or too low, subsequent crystallization will fail.
[0030] S200: Dissolve the nickel source compound in deionized water
[0031] In this step, the nickel source compound is dissolved in deionized water to obtain solution B. Specifically, the mass volume ratio of the nickel source compound to deionized water is (0.20-0.40) g: (10-30) mL. The inventors have found that when the ratio of each component is too high or too low, subsequent crystallization will fail.
[0032] It should be noted that the choice of nickel source compound is not particularly limited, and those skilled in the art can select it according to needs, including at least one of nickel nitrate hexahydrate, nickel acetate tetrahydrate, nickel sulfate hexahydrate and nickel chloride hexahydrate.
[0033] S300: Mix solution A and solution B evenly, put them into a reactor lined with polytetrafluoroethylene, place them in an oven for constant temperature crystallization, cool them to room temperature, centrifuge, wash and dry them
[0034] In this step, the above-mentioned solution A and solution B are mixed evenly, loaded into a reaction kettle lined with polytetrafluoroethylene, placed in an oven, and crystallized at a constant temperature of 90-120° C. for 48-96 hours. After cooling to room temperature, solid powder is obtained by centrifugation, washed thoroughly with deionized water and ethanol, and then dried at 80-100° C. for 8-12 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0035] According to the method for preparing a defective Ni-MOFs desulfurization adsorbent according to an embodiment of the present invention, a template agent N,N-dimethyloctadecylamine is added to a precursor solution with a nickel source and 2,5-dihydroxyterephthalic acid as raw materials, and a defective Ni-MOFs desulfurization adsorbent is prepared by a solvothermal method. After the template agent N,N-dimethyloctadecylamine is removed, uniformly distributed mesopores can be obtained. The defective Ni-MOFs desulfurization adsorbent prepared by this method retains a certain proportion of the original micropores, and its mesopore diameter can be expanded to 2-5nm, and has good stability. While removing the template agent, the unsaturated metal sites of the nickel core are increased, and a uniform mesopore distribution is introduced into the original microporous material, which promotes more unsaturated nickel active sites to be fully exposed. The large pore size is conducive to the mass transfer process, and the exposed unsaturated nickel active sites enhance the interaction with the sulfide, greatly improving the adsorption amount. These two advantages make defective Ni-MOFs have excellent adsorption properties for thiophene sulfides.
[0036] In the second aspect of the present invention, the present invention proposes a defective Ni-MOFs desulfurization adsorbent. According to an embodiment of the present invention, the defective Ni-MOFs desulfurization adsorbent is prepared by the above method. As a result, the defective Ni-MOFs desulfurization adsorbent has a uniform mesopore distribution and more unsaturated active sites, wherein the large pore size is conducive to the mass transfer process, and the exposed unsaturated nickel active sites enhance the interaction with the sulfide, greatly improving the adsorption amount. These two advantages make the defective Ni-MOFs desulfurization adsorbent have excellent adsorption performance for sulfides in oil products.
[0037] In the third aspect of the present invention, the present invention proposes an application of a defective Ni-MOFs desulfurization adsorbent. According to an embodiment of the present invention, the defective Ni-MOFs desulfurization adsorbent is prepared by the above method, and the above application includes the application of adsorption and removal of sulfides in oil products.
[0038] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0039] Example 1
[0040] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.2 g of template N,N-dimethyloctadecylamine in 10 mL of tetrahydrofuran to obtain solution A;
[0041] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0042] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0043] Example 2
[0044] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.28 g of template N,N-dimethyloctadecylamine in 10 mL of tetrahydrofuran to obtain solution A;
[0045] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0046] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0047] Example 3
[0048] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.28 g of template N,N-dimethyloctadecylamine in 10 mL of tetrahydrofuran to obtain solution A;
[0049] (2) dissolving 0.4 g of nickel source compound nickel nitrate hexahydrate in 10 mL of deionized water to obtain solution B;
[0050] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0051] Example 4
[0052] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.28 g of template N,N-dimethyloctadecylamine in 10 mL of tetrahydrofuran to obtain solution A;
[0053] (2) dissolving 0.4 g of nickel source compound nickel chloride hexahydrate in 10 mL of deionized water to obtain solution B;
[0054] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0055] Example 5
[0056] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.28 g of template N,N-dimethyloctadecylamine in 10 mL of tetrahydrofuran to obtain solution A;
[0057] (2) dissolving 0.4 g of nickel sulfate hexahydrate, a nickel source compound, in 10 mL of deionized water to obtain solution B;
[0058] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0059] Comparative Example 1
[0060] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid in 10 mL of tetrahydrofuran to obtain solution A;
[0061] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0062] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0063] Comparative Example 2
[0064] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.28 g of template agent hexadecyltrimethylammonium bromide in 10 mL of tetrahydrofuran to obtain solution A;
[0065] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0066] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0067] Comparative Example 3
[0068] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.28 g of template agent dodecanoic acid in 10 mL of tetrahydrofuran to obtain solution A;
[0069] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0070] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0071] Comparative Example 4
[0072] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.28 g of template agent dodecyloxybenzoic acid in 10 mL of tetrahydrofuran to obtain solution A;
[0073] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0074] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0075] Comparative Example 5
[0076] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.04 g of template N,N-dimethyloctadecylamine in 10 mL of tetrahydrofuran to obtain solution A;
[0077] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0078] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0079] Comparative Example 6
[0080] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.12 g of template N,N-dimethyloctadecylamine in 10 mL of tetrahydrofuran to obtain solution A;
[0081] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0082] The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain the defective Ni-MOFs desulfurization adsorbent.
[0083] Comparative Example 7
[0084] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.32 g of template N,N-dimethyloctadecylamine in 10 mL of tetrahydrofuran to obtain solution A;
[0085] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0086] (3) The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain a defective Ni-MOFs desulfurization adsorbent.
[0087] Comparative Example 8
[0088] (1) dissolving 0.16 g of ligand 2,5-dihydroxyterephthalic acid and 0.4 g of template N,N-dimethyloctadecylamine in 10 mL of tetrahydrofuran to obtain solution A;
[0089] (2) dissolving 0.4 g of nickel source compound nickel acetate tetrahydrate in 10 mL of deionized water to obtain solution B;
[0090] The two solutions were mixed and loaded into a polytetrafluoroethylene-lined reactor, and crystallized at 100°C for 72 hours. After the crystallization was completed, solid powder was obtained by centrifugation, and then fully washed with deionized water and ethanol. After centrifugation, it was dried at 80°C for 10 hours to obtain the defective Ni-MOFs desulfurization adsorbent.
[0091] Fixed bed desulfurization test: On a fixed bed device, the desulfurization adsorbents of Examples 1 to 5 and Comparative Examples 1 to 8 were used to carry out adsorption desulfurization of n-octane containing thiophene, that is, adsorption performance evaluation. The content of each component in the mixed liquid fuel is as follows: benzothiophene: 100ppmw, n-octane balance. The desulfurization adsorption evaluation experimental conditions of the adsorbent are: at a temperature of 30°C, a pressure of 1 bar, and a liquid flow rate of 2mL / min, the simulated fuel is adsorbed and purified by loading a defective Ni-MOFs desulfurization adsorbent to obtain purified n-octane. The evaluation results of breakthrough sulfur capacity, saturated sulfur capacity, and fuel oil processing capacity are given in Table 1.
[0092] Table 1 Addition amount of each component of the embodiment and comparative example and fixed bed desulfurization test results
[0093]
[0094] From the comparison results of the examples and comparative examples, it can be seen that compared with other templates, N,N-dimethyloctadecylamine as a template has a better desulfurization effect. In the process of preparing defective Ni-MOFs desulfurization adsorbent, first, N,N-dimethyloctadecylamine molecules self-assemble into supramolecular micelles in the solution, and the H + Combined with the amino group of the template under the interaction of charges; then the nickel source solution is added to the reaction system, the organic ligand and Ni 2+ Self-assembled on the outer surface of micelles, MOFs with microporous and mesoporous structural skeletons were constructed; finally, when the template was removed by heating, mesopores were formed in the framework of defective Ni-MOFs. N,N-dimethyloctadecylamine was selected as the template, which has better interaction with the precursors (metal ions and organic ligands) of defective Ni-MOFs, thus achieving better desulfurization effect.
[0095] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0096] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a defective Ni-MOFs desulfurization adsorbent, characterized in that: The following steps are involved: (1) dissolving 2,5-dihydroxyterephthalic acid and N,N-dimethyloctadecylamine in tetrahydrofuran to obtain a solution A; (2) dissolving the nickel source compound in deionized water to obtain solution B; (3) mixing the solution A and the solution B evenly, loading them into a reactor lined with polytetrafluoroethylene, placing them in an oven for constant temperature crystallization, cooling them to room temperature, centrifuging, washing and drying them to obtain a defective Ni-MOFs desulfurization adsorbent; The mass volume ratio of the 2,5-dihydroxyterephthalic acid, the N,N-dimethyloctadecylamine, the nickel source compound, the tetrahydrofuran and the deionized water is (0.10-0.20) g: (0.20-0.28) g: (0.20-0.40) g: (10-30) mL: (10-30) mL; In step (3), the crystallization temperature is 90 to 120° C. and the crystallization time is 48 to 96 h.
2. The method according to claim 1, characterized in that In step (2), the nickel source compound includes at least one of nickel nitrate hexahydrate, nickel acetate tetrahydrate, nickel sulfate hexahydrate and nickel chloride hexahydrate.
3. The method according to claim 1, characterized in that In step (3), the drying temperature is 80-100° C. and the drying time is 8-12 h.
4. The method according to claim 1, characterized in that: In step (3), the washing includes: first washing with deionized water and then washing with ethanol.
5. A defective Ni-MOFs desulfurization adsorbent, characterized in that: The defective Ni-MOFs desulfurization adsorbent is prepared by the method according to any one of claims 1 to 4.
6. An application of defective Ni-MOFs desulfurization adsorbent, characterized in that: The defective Ni-MOFs desulfurization adsorbent is prepared by the method described in any one of claims 1 to 4, and the application includes the application of adsorption and removal of sulfides in oil products.