A hierarchical intelligent induction wood floor and preparation method thereof

Through supercritical pretreatment, high-temperature steam softening and compression, temperature intelligent sensing modifier impregnation and vacuum drying processes, combined with phase change energy storage material processing of the base material, a graded intelligent induction wood floor that can intelligently respond to changes in ambient temperature is prepared. It solves the problem that existing wooden floors cannot effectively respond to temperature changes, and improves user experience and energy efficiency.

CN115741929BActive Publication Date: 2024-10-01GUANGDONG NATURE HOME FURNISHING TECH RES CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211413510.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-11
Publication Date
2024-10-01
Estimated Expiration
2042-11-11

AI Technical Summary

Technical Problem

Existing wooden floors cannot effectively respond to changes in ambient temperature, resulting in poor user experience and comfort.

Method used

Using supercritical pretreatment, high-temperature steam softening and compression, temperature smart sensing modifier impregnation and vacuum drying processes, combined with phase change energy storage material processing of the base material, a hierarchical smart sensing wood floor is prepared, allowing it to intelligently respond to ambient temperature change.

Benefits of technology

It realizes the intelligent response of the wooden floor to the ambient temperature, improves the safety and comfort of the product, and has beautiful decorative properties and early warning functions to alleviate the impact of external temperature changes on the indoor environment and save energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003939672890000211
    Figure BDA0003939672890000211
Patent Text Reader

Abstract

The present invention discloses a graded intelligent inductive wood floor and a preparation method thereof, the preparation method comprising the following steps: (1) performing supercritical pretreatment on veneer; (2) performing high-temperature steam softening and compression treatment on the veneer treated in step (1); (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent inductive modifier for expansion treatment; (4) performing vacuum drying treatment on the veneer treated in step (3) to obtain modified veneer; (5) coating a layer of adhesive on the surface of a substrate, and then pressing and molding with the modified veneer to obtain a graded intelligent inductive wood floor; wherein the temperature intelligent inductive modifier comprises a temperature-sensitive color-changing material and crystal violet lactone. The present invention also provides a graded intelligent inductive wood floor. The wood floor prepared by the present invention can realize intelligent response to ambient temperature and play a certain early warning role.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flooring, and in particular to a graded intelligent induction wood floor and a preparation method thereof. Background Art

[0002] Color and texture are important factors that affect the commercial value of wood. Improving the color and functional properties of wood can significantly increase the added value of products. On the basis of saving wood resources, it can meet the diverse decorative requirements of consumers. By improving the visual characteristics and decorative properties of low-grade solid wood, fiberboard, plywood, blockboard and other substrates with damaged appearance textures, the natural appearance defects of wood can be eliminated. At the same time, the use value of low-quality wood can be improved by imitating the color of precious wood.

[0003] Existing wooden floors usually have anti-slip and waterproof functions, but cannot respond to changes in ambient temperature in a timely manner, resulting in poor user experience and comfort. Therefore, there is an urgent need to find an intelligent sensing wooden floor that can respond to temperature changes in a timely manner. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a graded intelligent induction wood floor and a preparation method thereof, wherein the prepared wood floor can realize an intelligent response to changes in ambient temperature and play a certain early warning role.

[0005] In order to solve the above technical problems, the present invention provides a method for preparing a graded intelligent induction wooden floor, comprising the following steps:

[0006] (1) supercritical pretreatment of veneer;

[0007] (2) subjecting the veneer treated in step (1) to high temperature steam softening and compression treatment;

[0008] (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent sensing modifier for expansion treatment;

[0009] (4) vacuum drying the veneer treated in step (3) to obtain modified veneer;

[0010] (5) coating a layer of adhesive on the surface of the substrate, and then pressing and molding with the modified veneer to obtain a graded intelligent induction wood floor;

[0011] Wherein, the temperature intelligent sensing modifier includes a temperature-sensitive color-changing material and crystal violet lactone.

[0012] As an improvement of the above scheme, the temperature intelligent sensing modifier includes 25-85 parts of A modified solution, 18-75 parts of B modified solution and 0.5-1.2 parts of defoaming agent calculated by volume;

[0013] The raw materials for preparing the modified solution A include 0.8-4 parts by mass of a temperature-sensitive color-changing material, 5-9 parts by volume of a first solvent, 4-7 parts by volume of a silane crosslinking agent, 3-6 parts by volume of a silane coupling agent, 1-5 parts by volume of ammonia water, 40-80 parts by volume of deionized water, and 10-30 parts by volume of nanofibrillated cellulose;

[0014] The raw materials for preparing the B modified solution include 50-80 parts by volume of isocyanate, 10-25 parts by volume of polyethylene glycol, 70-90 parts by volume of a second solvent, 4-8 parts by volume of a chain extender, 20-40 parts by volume of a modified crystal violet lactone, 1-2.8 parts by volume of a catalyst, 5.4-10 parts by volume of a capping agent, 1-5 parts by volume of a salt-forming agent, 70-85 parts by volume of deionized water and 1-5 parts by volume of an emulsifier;

[0015] The temperature-sensitive color-changing material is one or more of silver mercury iodide and copper mercury iodide.

[0016] As an improvement of the above scheme, the crystal violet lactone is a modified crystal violet lactone, and the preparation method of the modified crystal violet lactone is:

[0017] 1.5-3 parts by mass of crystal violet lactone is dissolved in 3-10 parts by volume of a third solvent, subjected to ultrasonic treatment for 10-30 minutes, and 1-5 parts by volume of hydrogen bromide is added and reacted at room temperature for 20-80 minutes to obtain a mixed solution;

[0018] Adding sodium hydroxide with a mass concentration of 20-40% to the mixed solution for hydrolysis, and then washing with deionized water for 3-5 times to obtain modified crystal violet lactone;

[0019] Wherein, the amount of sodium hydroxide added is 20-50% of the volume of the mixed solution;

[0020] The third solvent is one or more of isopropanol, toluene, methanol, ethanol, dichloromethane, and acetone.

[0021] As an improvement of the above scheme, the preparation method of the A modified solution is:

[0022] 0.8-4 parts by mass of a thermochromic material and 5-9 parts by volume of a first solvent are ultrasonically dispersed at 55-65° C. for 30-60 minutes, and then 4-7 parts by volume of a silane crosslinking agent, 3-6 parts by volume of a silane coupling agent, 1-5 parts by volume of ammonia water and 40-80 parts by volume of deionized water are added, and stirred at 70° C. for 1.5-3 hours, and then 10-30 parts by volume of nanofibrillated cellulose with a mass concentration of 0.8%-1.5% is added, and ultrasonicated at 70-80° C. for 30 minutes to obtain a modified solution A;

[0023] Wherein, the first solvent is one or more of isopropanol, toluene, methanol, ethanol, dichloromethane, and acetone;

[0024] The silane crosslinking agent is one or more of ethyl orthosilicate, methyltriacetoxysilane, methyltrimethoxysilane, and methyltributylidene oxime silane;

[0025] The silane coupling agent is one or more of 3-aminopropyltriethoxysilane, tributylaminomethylsilane, γ-aminoethylaminopropyltrimethoxysilane, and N-aminoethyl-3-aminopropylmethyldimethoxysilane.

[0026] As an improvement of the above scheme, the preparation method of the B modified solution is:

[0027] In an argon protective environment, add 50-80 parts by volume of isocyanate, 10-25 parts by volume of polyethylene glycol and 70-90 parts by volume of the second solvent at 45-60°C, mix well; then heat to 70-80°C and stir for 30-45min, slowly drop 4-8 parts by volume of chain extender, 20-40 parts by volume of modified crystal violet lactone and 1-2.8 parts by volume of catalyst, react at 75°C-80°C for 2-3h; then add 5.4-10 parts by volume of end-capping agent, heat to 85°C and keep for 30min; cool to 40-60°C, add 1-5 parts by volume of salt-forming agent, keep for 15-40min, add 70-85 parts by volume of deionized water and 1-5 parts by volume of emulsifier for emulsification and dispersion, and obtain B modified solution;

[0028] The isocyanate is one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate;

[0029] The second solvent is one or more of benzene, toluene, carbon tetrachloride, acetone, ethyl acetate, dimethyl sulfoxide, chloroform, N,N-dimethylformamide and N,N-dimethylacetamide;

[0030] The chain extender is one or more of 2,2-dimethylol propionic acid, dihydroxy half ester, sodium ethylenediaminoethanesulfonate, diethylenetriamine or methyldiethanolamine;

[0031] The catalyst is one or more of dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, stannous octoate, dimethyltin dineodecanoate, and dibutyltin bis(β-diketonate);

[0032] The end-capping agent is caprolactam;

[0033] The salt-forming agent is one or more of triethylamine, hydrochloric acid, acetic acid and propylene oxide.

[0034] As an improvement of the above scheme, the preparation method of the temperature intelligent sensing modifier is:

[0035] Calculated by volume, 25-85 parts of modified solution A and 18-75 parts of modified solution B are mixed, and then 0.5-1.2 parts of defoaming agent are added, and stirred at 450-1000 rpm for 30-90 minutes at 45-70°C to obtain a temperature intelligent sensing modifier.

[0036] As an improvement of the above scheme, step (1) includes:

[0037] (11) The supercritical fluid is carbon dioxide, and a benzene-ethanol solution is used as an entrainer to perform a first supercritical pretreatment on the veneer; wherein the supercritical temperature is 35-45° C., the pressure is 10-30 MPa, the time is 30-100 min, and the flow rate is 10 -40 L / h;

[0038] (12) After the first supercritical pretreatment, maleic anhydride is added and dissolved in the carbon dioxide fluid to obtain a mixed solution, and the veneer is subjected to a second supercritical pretreatment; wherein the supercritical temperature is 50-65° C., the pressure is 8-15 MPa, the time is 60-120 min, and the flow rate is 10-30 L / h;

[0039] The amount of maleic anhydride added is 30-75% of the mass of the mixed solution.

[0040] As an improvement of the above solution, the thickness of the veneer is 1.0-3.0 mm;

[0041] The temperature of step (2) is 100-120°C, the compression rate is set to 50-70%, and the unit hot pressing pressure is 1.5-3MPa / m 2 , hot pressing time is 5-20min;

[0042] Step (3) setting the expansion rate to 60-90%, the temperature to 40-65° C., and the mass concentration of the temperature intelligent sensing modifier in the atomization environment to 80-100%;

[0043] The temperature of step (4) is 35-45°C.

[0044] As an improvement of the above solution, the substrate is a modified substrate;

[0045] The modified substrate is prepared by the following method:

[0046] The substrate is placed in a sealed impregnation tank, and the vacuum is drawn to a vacuum degree of -(0.090-0.097) MPa for 25-35 minutes. The pre-configured modified isocyanate solution is introduced under vacuum, and the substrate is subjected to pressurized impregnation treatment, with an impregnation pressure of 2.5-4 MPa and an impregnation time of 3-5 hours. The modified isocyanate solution is discharged after the pressure is released every 60 minutes, and then the pressure is re-applied to obtain a modified substrate;

[0047] The modified isocyanate solution comprises 2-10 parts by mass of phase change energy storage microcapsules, 15-35 parts by volume of a wet strength agent, 20-50 parts by volume of sodium silicate and 40-68 parts by volume of modified isocyanate;

[0048] The mass concentration of the wet strength agent is 18-20%, and the mass concentration of the sodium silicate is 35-45%;

[0049] The graded intelligent induction wooden floor is also provided with a waterproof layer and a wear-resistant layer.

[0050] Correspondingly, the present invention also provides a graded intelligent induction wood floor, which is prepared by the above-mentioned preparation method of the graded intelligent induction wood floor.

[0051] The implementation of the present invention has the following beneficial effects:

[0052] 1. The preparation method of the graded intelligent induction wood floor provided by the present invention is to perform supercritical-high temperature compression-temperature intelligent induction modifier impregnation-vacuum drying processes on the veneer, and then composite it with the substrate to form a graded intelligent induction wood floor. The prepared wood floor can realize intelligent response to changes in ambient temperature, play a certain early warning role, improve the safety of product use, and at the same time enrich the consumer's visual experience and comfort of use.

[0053] 2. The graded intelligent sensing wooden floor provided by the present invention has a surface veneer modified with a temperature intelligent sensing modifier and has a multi-level color change system. When the ambient temperature is in different temperature ranges, the wooden floor presents different colors, which can achieve an intelligent response to the ambient temperature, so that the wooden floor has beautiful decorative performance and early warning function; the base material is modified with a phase change energy storage material to play a role in regulating the ambient temperature, alleviate the impact of rapid changes in external temperature on the indoor environment, improve the comfort of the use environment, and save energy. DETAILED DESCRIPTION

[0054] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.

[0055] In order to solve the above technical problems, the present invention provides a method for preparing a graded intelligent induction wooden floor, comprising the following steps:

[0056] S1: supercritical pretreatment of veneer;

[0057] Specifically, step S1 also includes:

[0058] S11: placing the veneer in a supercritical device, wherein the supercritical fluid is carbon dioxide and a benzene-ethanol solution is used as an entrainer, and performing a first supercritical pretreatment on the veneer;

[0059] The supercritical temperature of step S11 is 35-45°C, the pressure is 10-30 MPa, the time is 30-100 min, and the flow rate is 10-40 L / h. Preferably, the supercritical temperature of step S1 is 35-42°C, the pressure is 15-28 MPa, the time is 30-90 min, and the flow rate is 15-40 L / h.

[0060] The present invention performs a first supercritical pretreatment on the veneer, which, on the one hand, forms a pressure difference between the inside and outside of the veneer to cause the pit membrane to rupture, and on the other hand, uses an entrainer to dissolve part of the extract to improve its permeability, so that the subsequent temperature intelligent sensing modifier is more evenly distributed in the veneer, and the color change of the veneer is more significant.

[0061] S12: After the first supercritical pretreatment, maleic anhydride is added and dissolved in the carbon dioxide fluid to obtain a mixed solution, and the veneer is subjected to a second supercritical pretreatment;

[0062] The temperature of step S12 is 50-65°C, the pressure is 8-15 MPa, the time is 60-120 min, and the flow rate is 10-30 L / h. Preferably, the temperature of step S2 is 50-60°C, the pressure is 9-12 MPa, the time is 65-120 min, and the flow rate is 12-30 L / h.

[0063] Specifically, the thickness of the veneer is 1.0-3.0 mm, preferably 1.2-2.5 mm, and exemplary ones are 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.85 mm, 1.9 mm, 1.95 mm, 2.0 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, and 2.5 mm, but are not limited to these.

[0064] The amount of maleic anhydride added is 30-75% of the mass of the mixed solution, preferably 40-75%. If the amount of maleic anhydride added is too little, the veneer cannot be effectively modified, and the obtained modified veneer has poor temperature intelligent sensitivity and thermal stability; if the amount of maleic anhydride added is too much, the subsequent temperature intelligent sensitivity modifier will have an adverse effect on the modification of the veneer.

[0065] The present invention uses maleic anhydride to perform interface modification treatment on veneer. Maleic anhydride reacts with hydroxyl groups in the veneer to form chemical bonds. In the subsequent process of adding a temperature intelligent sensing modifier, it plays a role of chemical coupling, enhances the compatibility of the veneer and the temperature intelligent sensing modifier, and further improves the temperature intelligent sensitivity and thermal stability of the composite wood flooring product.

[0066] S2: subjecting the veneer treated in step S1 to high temperature steam softening and compression treatment;

[0067] The temperature is 100-120℃, the compression rate is 50-70%, and the unit hot pressing pressure is 1.5-3MPa / m 2 , the hot pressing time is 5-20min. Preferably, the temperature is 105-120°C, the compression rate is set to 55-70%, and the unit hot pressing pressure is 2-3MPa / m 2 , hot pressing time is 8-20min.

[0068] The present invention uses high-temperature steam to perform high-temperature softening treatment on the veneer, and at the same time cooperates with compression treatment, which can lay a foundation for the subsequent veneer to absorb the temperature intelligent sensing modifier, thereby improving the veneer's absorption rate of the modifier, and further improving the temperature intelligent sensitivity of the wood floor product.

[0069] S3: placing the veneer treated in step S2 in an atomized environment of a temperature intelligent sensing modifier for expansion treatment;

[0070] The expansion rate is set to 60-90%, the temperature is set to 40-65° C., and the mass concentration of the temperature intelligent sensing modifier in the atomization environment is set to 80-100%.

[0071] Specifically, calculated by volume, the temperature intelligent sensing modifier includes 25-85 parts of A modified solution, 18-75 parts of B modified solution and 0.5-1.2 parts of defoaming agent;

[0072] The raw materials for preparing the modified solution A include 0.8-4 parts by mass of a temperature-sensitive color-changing material, 5-9 parts by volume of a first solvent, 4-7 parts by volume of a silane crosslinking agent, 3-6 parts by volume of a silane coupling agent, 1-5 parts by volume of ammonia water, 40-80 parts by volume of deionized water and 10-30 parts by volume of nanofibrillated cellulose (NFC); ​​wherein 1 part by mass: 1 part by volume = 1 g: 1 ml.

[0073] The temperature-sensitive color-changing material is one or more of mercuric silver iodide and mercuric copper iodide, but is not limited thereto. Different temperature-sensitive color-changing materials can be selected according to user needs and environmental conditions. Preferably, in some embodiments of the present invention, the temperature-sensitive color-changing material is mercuric silver iodide, and the wooden floor produced therefrom has a three-level color-changing system of room temperature, 30-40°C, and 70-80°C.

[0074] The preparation method of A modified solution is as follows:

[0075] Take 0.8-4 parts by mass of the thermochromic material and 5-9 parts by volume of the first solvent, and ultrasonically disperse them at 55-65° C. for 30-60 minutes. Then add 4-7 parts by volume of a silane crosslinker, 3-6 parts by volume of a silane coupling agent, 1-5 parts by volume of ammonia water and 40-80 parts by volume of deionized water. Stir at 70° C. for 1.5-3 hours. Then add 10-30 parts by volume of nanofibrillated cellulose with a mass concentration of 0.8%-1.5%, and ultrasonicate at 70-80° C. for 30 minutes to obtain a modified solution A.

[0076] Wherein, the first solvent is one or more of isopropanol, toluene, methanol, ethanol, and dichloromethane, preferably isopropanol.

[0077] The silane crosslinking agent is one or more of tetraethyl orthosilicate, methyltriacetoxysilane, methyltrimethoxysilane, and methyltributylidene oxime silane, preferably tetraethyl orthosilicate.

[0078] The silane coupling agent is one or more of 3-aminopropyltriethoxysilane, tributylaminomethylsilane, γ-aminoethylaminopropyltrimethoxysilane, and N-aminoethyl-3-aminopropylmethyldimethoxysilane, preferably 3-aminopropyltriethoxysilane.

[0079] The present invention embeds and fixes silver mercury iodide on nano-fibrillated cellulose (NFC) by means of sol, which can effectively enhance the thermal stability of the NFC.

[0080] The raw materials for preparing the B modified solution include 50-80 parts by volume of isocyanate, 10-25 parts by volume of polyethylene glycol, 70-90 parts by volume of a second solvent, 4-8 parts by volume of a chain extender, 20-40 parts by volume of a modified crystal violet lactone, 1-2.8 parts by volume of a catalyst, 5.4-10 parts by volume of a capping agent, 1-5 parts by volume of a salt-forming agent, 70-85 parts by volume of deionized water and 1-5 parts by volume of an emulsifier; wherein 1 part by mass: 1 part by volume = 1 g: 1 ml.

[0081] The preparation method of B modified solution is as follows:

[0082] In an argon protective environment, add 50-80 parts by volume of isocyanate, 10-25 parts by volume of polyethylene glycol and 70-90 parts by volume of the second solvent at 45-60° C. and mix well; then heat to 70-80° C. and stir for 30-45 minutes, slowly drop 4-8 parts by volume of a chain extender, 20-40 parts by volume of a modified crystal violet lactone and 1-2.8 parts by volume of a catalyst, and react at 75° C.-80° C. for 2-3 hours; then add 5.4-10 parts by volume of a capping agent, heat to 85° C. and keep for 30 minutes; cool to 40-60° C., add 1-5 parts by volume of a salt-forming agent, keep for 15-40 minutes, add 70-85 parts by volume of deionized water and 1-5 parts by volume of an emulsifier for emulsification and dispersion, and obtain a B modified solution.

[0083] The isocyanate is one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate, preferably diphenylmethane diisocyanate.

[0084] The second solvent is one or more of benzene, toluene, carbon tetrachloride, acetone, ethyl acetate, dimethyl sulfoxide, chloroform, N,N-dimethylformamide and N,N-dimethylacetamide, preferably toluene.

[0085] The chain extender is one or more of 2,2-dimethylol propionic acid, dihydroxy half ester, sodium ethylenediaminoethanesulfonate, diethylenetriamine or methyldiethanolamine, preferably 2,2-dimethylol propionic acid.

[0086] The catalyst is one or more of dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, stannous octoate, dimethyltin diceneodecanoate, and dibutyltin bis(β-diketone ester), preferably dibutyltin dilaurate.

[0087] The end-capping agent is caprolactam.

[0088] The salt-forming agent is one or more of triethylamine, hydrochloric acid, acetic acid, and propylene oxide, preferably triethylamine.

[0089] Wherein, the crystal violet lactone is a modified crystal violet lactone, and the preparation method of the modified crystal violet lactone is:

[0090] 1.5-3 parts by mass of crystal violet lactone is dissolved in 3-10 parts by volume of a third solvent, subjected to ultrasonic treatment for 10-30 minutes, and 1-5 parts by volume of hydrogen bromide is added and reacted at room temperature for 20-80 minutes to obtain a mixed solution;

[0091] Adding sodium hydroxide with a mass concentration of 20-40% to the mixed solution for hydrolysis, and then washing with deionized water for 3-5 times to obtain modified crystal violet lactone;

[0092] Wherein, the amount of sodium hydroxide added is 20-50% of the volume of the mixed solution;

[0093] The third solvent is one or more of isopropanol, toluene, methanol, ethanol, and dichloromethane, preferably isopropanol.

[0094] The temperature intelligent sensing modifier used in the present invention mainly includes a graded intelligent temperature response composed of organic and inorganic synergistic system of thermochromic materials. The inorganic thermochromic material is silanized and embedded and fixed on nano-fibrillated cellulose (NFC) by a sol method, which effectively enhances the thermal stability of the thermochromic material and is beneficial to uniform impregnation and uniform color change in the veneer. The combination of thermochromic materials of different colors also increases the color change range, making the color change between cold and warm tones more obvious.

[0095] After the crystal violet lactone is subjected to the above-mentioned modification treatment, the present invention is conducive to the subsequent reaction between the modified crystal violet lactone and the polyurethane chain segment, thereby effectively improving the performance of the prepared temperature intelligent sensing modifier.

[0096] Furthermore, the present invention introduces the dye functional monomer, modified crystal violet lactone, into the polyurethane chain segment to synthesize a modified waterborne polyurethane dispersion, which can effectively reduce its volatility and improve the safety of the prepared modified veneer. At the same time, it makes the color change faster, weakens the hysteresis phenomenon, and greatly improves the stability and durability of the use environment.

[0097] In addition, the present invention makes full use of the rebound characteristics of the compressed veneer. By immersing the veneer treated with high-temperature steam compression in an atomized environment of the temperature intelligent sensing modifier, it helps to improve the uniformity and depth of deposition of the temperature intelligent sensing modifier inside the wood and increase the retention rate.

[0098] Furthermore, the preparation method of the temperature intelligent sensing modifier is:

[0099] Calculated by volume, 25-85 parts of modified solution A and 18-75 parts of modified solution B are mixed, and then 0.5-1.2 parts of defoaming agent are added, and stirred at 450-1000 rpm for 30-90 minutes at 45-70°C to obtain a temperature intelligent sensing modifier.

[0100] S4: vacuum drying the veneer treated in step S3 to obtain modified veneer;

[0101] The treatment temperature is 35-45°C, preferably 35-40°C.

[0102] The present invention can quickly combine the temperature intelligent sensing modifier with the veneer by vacuum drying the veneer impregnated with the temperature intelligent sensing modifier, thereby ensuring the temperature intelligent responsiveness and thermal stability of the modified veneer. The prepared wooden floor can achieve intelligent response to the ambient temperature, play a certain early warning role, improve the safety of product use, and at the same time enrich the visual experience and comfort of consumers.

[0103] The surface veneer of the present invention is modified with a temperature intelligent sensing modifier and has a multi-stage color changing system. The wooden floor presents different colors when the ambient temperature is in different temperature ranges, and can achieve intelligent response to the ambient temperature, so that the wooden floor has beautiful decorative performance and early warning function; at the same time, different proportions can also form different colors, enriching the color of the intelligent response wooden floor product.

[0104] S5: A layer of adhesive is coated on the surface of the substrate, and then pressed together with the modified veneer to form a graded intelligent induction wooden floor.

[0105] Specifically, the substrate is a modified substrate, and the modified substrate is prepared by the following method:

[0106] The substrate is placed in a sealed impregnation treatment tank, and the vacuum degree in the tank is -(0.090-0.097)MPa, and the holding time is 25-35min. The pre-configured modified isocyanate solution is introduced under vacuum, and the substrate is subjected to pressurized impregnation treatment, the impregnation pressure is 2.5-4MPa, and the impregnation time is 3-5h. The modified isocyanate solution is discharged after the pressure is released every 60min, and then the pressure is re-applied to obtain a modified substrate;

[0107] The modified isocyanate solution comprises 2-10 parts by mass of phase change energy storage microcapsules, 15-35 parts by volume of wet strength agent, 20-50 parts by volume of sodium silicate and 40-68 parts by volume of modified isocyanate; wherein 1 part by mass: 1 part by volume = 1 g: 1 ml.

[0108] The mass concentration of the wet strength agent is 18-20%, and the mass concentration of the sodium silicate is 35-45%.

[0109] The present invention adopts the above treatment to adsorb and fix the modified isocyanate solution inside the substrate, reduce leakage, further enrich the energy storage performance of the product, and effectively enhance the density and strength of the substrate. The substrate is modified by using phase change energy storage material to regulate the ambient temperature, alleviate the impact of rapid changes in external temperature on the indoor environment, improve the comfort of the use environment, and save energy.

[0110] Preferably, in some embodiments of the present invention, the substrate is a five-layer solid wood composite substrate, and the middle layer is 10-13mm thick pine wood. More preferably, a high thermal conductivity film is also provided on the sub-surface and sub-bottom of the five-layer solid wood composite substrate to improve the thermal conductivity and thermal uniformity of the board, thereby saving the thermal conductivity cost of floor heating, achieving a warm winter and cool summer living environment and low-carbon and environmentally friendly, and can synergistically enhance the temperature response color change effect of graded intelligent sensing wood flooring; at the same time, the dimensional stability of the substrate is improved, and compared with the prior art, the appearance of rib patterns during use is avoided, and the deformation of the floor and cracking of the surface are reduced. Specifically, the high thermal conductivity film is model KGF080 of Shenzhen Hanhua Thermal Management Technology Co., Ltd., but is not limited to this.

[0111] Preferably, in some embodiments of the present invention, the graded intelligent induction wooden floor is further provided with a waterproof layer. Specifically, the graded intelligent induction wooden floor is immersed in a silicone waterproofing agent for 5-15 minutes and repeated 1-3 times. In this way, a waterproof layer can be coated on the surface of the graded intelligent induction wooden floor, thereby improving the waterproof performance of the graded intelligent induction wooden floor.

[0112] Preferably, in some embodiments of the present invention, a layer of adhesive waterproof wood wax oil is coated on the surface of the graded intelligent induction wooden floor coated with a waterproof layer, which can further improve its waterproof performance.

[0113] Preferably, in some embodiments of the present invention, the graded intelligent induction wooden floor is also provided with a wear-resistant layer, and alumina wear-resistant particles are deposited on the surface of the graded intelligent induction wooden floor by magnetron sputtering to construct a hydrophobic wear-resistant layer. Specifically, the sputtering power is 100W in an argon atmosphere, the sputtering pressure is 1.5-2.5MPa, and the sputtering time is 60-200min. Finally, freeze-drying is performed to achieve paint-free decoration on the surface of the wooden floor, improve the surface effect and performance of the board, and make it more low-carbon and environmentally friendly.

[0114] The hierarchical intelligent induction wood floor of the present invention retains the beautiful and elegant natural texture of the wood itself, and at the same time, the temperature intelligent induction color change enriches the visual enjoyment of the user, and on a certain basis, plays a high temperature warning function of the wood floor to prevent safety hazards caused by local high temperature. Therefore, the hierarchical intelligent induction wood floor of the present invention is particularly suitable for floor heating wood floor.

[0115] Correspondingly, the present invention also provides a graded intelligent induction wood floor, which is prepared by the preparation method of the graded intelligent induction wood floor.

[0116] The present invention is further described below with specific embodiments:

[0117] The sources of some raw materials in the examples are as follows, but are not limited to these raw materials:

[0118] The nanofibrillated cellulose (NFC) used was NFC-H1 from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.;

[0119] The phase change energy storage microcapsule used is RX-xb001 from Hefei Ruixue New Materials Technology Co., Ltd.;

[0120] The wet strength agent used was JN PPE-1101 from Junneng Chemical (Longnan) Co., Ltd.;

[0121] The modified isocyanate used is from Wanhua Chemical Group Co., Ltd. 8617.

[0122] Example 1

[0123] Preparation of temperature intelligent sensing modifier:

[0124] Dissolve 50 g of silver mercury iodide in 375 ml of isopropanol, then add 50 g of crystal violet lactone and mix, and stir for 60 minutes to obtain a temperature intelligent sensing modifier.

[0125] A preparation method of graded intelligent induction wood floor:

[0126] (1) Select 1.6 mm veneer and place it in a supercritical device. The supercritical fluid is carbon dioxide and benzene-ethanol solution is used as an entrainer. The veneer is supercritically pretreated. The supercritical temperature is set to 38°C, the pressure is 18 MPa, the time is 60 min, and the flow rate is 18 L / h;

[0127] (2) The veneer treated in step (1) is placed in a press for 110°C high-temperature steam softening and compression treatment, with a compression rate of 60% and a hot pressing pressure of 2 MPa / m 2 , time is 5min;

[0128] (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent sensing modifier for expansion treatment, wherein the expansion rate is 75%, the temperature is 50° C., and the mass concentration of the temperature intelligent sensing modifier in the atomized environment is 80%;

[0129] (4) subjecting the veneer treated in step (3) to vacuum drying at a temperature of 40° C. to obtain modified veneer;

[0130] (5) A layer of PUR hot melt adhesive is coated on the surface of the substrate, and then it is pressed with the modified veneer to form a graded intelligent induction wooden floor; the graded intelligent induction wooden floor is immersed in a silicone waterproofing agent for 10 minutes, and alumina wear-resistant particles are deposited on the surface of the graded intelligent induction wooden floor by a magnetron sputtering method to construct a hydrophobic wear-resistant layer. Specifically, the sputtering power is 100 W, the sputtering pressure is 1.8 MPa, and the sputtering time is 100 minutes in an argon atmosphere. Finally, freeze-drying is performed to obtain a finished product.

[0131] The substrate is a modified substrate, which is prepared by the following method: placing the substrate in a closed impregnation treatment tank, evacuating the tank to a vacuum degree of -0.095 MPa, and maintaining the vacuum for 30 minutes, introducing a pre-configured modified isocyanate solution under vacuum, and performing pressurized impregnation treatment on the substrate, with an impregnation pressure of 3 MPa and an impregnation time of 4 hours, wherein the modified isocyanate solution is discharged after depressurization every 60 minutes, and then re-pressurized to obtain the modified substrate; the substrate adopts a five-layer solid wood composite substrate;

[0132] The modified isocyanate solution includes 100g of phase change energy storage microcapsules, 800ml of wet strength agent, 850ml of sodium silicate and 1250ml of modified isocyanate;

[0133] The mass concentration of the wet strength agent is 20%, and the mass concentration of the sodium silicate is 40%.

[0134] Example 2

[0135] Preparation of B modified solution:

[0136] In an argon protective environment, add 750 ml of MDI250, 187 g of PEG800 and 1000 ml of toluene solution at 45 ° C, heat to 75 ° C and stir for 35 minutes, slowly add 45 g of 2,2-dihydroxymethylpropionic acid, 200 ml of modified crystal violet lactone and 14 g of dibutyltin dilaurate, react at 80 ° C for 2 hours, add 58 g of caprolactam, heat to 85 ° C and keep for 30 minutes, cool to 45 ° C and add 20 ml of triethylamine and keep for 20 minutes, add 780 ml of deionized water and 30 ml of OP-10 emulsifier for emulsification and dispersion, and obtain B modified liquid.

[0137] The modified crystal violet lactone is prepared by the following method: 80 g of crystal violet lactone is dissolved in 200 ml of isopropanol, ultrasonically treated for 15 min, 40 ml of hydrogen bromide is added to react at room temperature for 30 min, then 70 ml of 30% mass concentration of sodium hydroxide is added for hydrolysis, and deionized water is used for washing 3 times to obtain the modified crystal violet lactone.

[0138] Preparation of temperature intelligent sensing modifier:

[0139] Dissolve 48 g of silver mercury iodide in 280 ml of isopropanol, then add 850 ml of modified solution B and mix, stir for 60 minutes to obtain a temperature intelligent sensing modifier.

[0140] A preparation method of graded intelligent induction wood floor:

[0141] (1) Select 1.6 mm veneer and place it in a supercritical device. The supercritical fluid is carbon dioxide and benzene-ethanol solution is used as an entrainer. The veneer is supercritically pretreated. The supercritical temperature is set to 40°C, the pressure is set to 20 MPa, the time is set to 60 min, and the flow rate is set to 22 L / h;

[0142] (2) The veneer treated in step (1) is placed in a press for 120°C high-temperature steam softening and compression treatment, with a compression rate of 60% and a hot pressing pressure of 2 MPa / m 2 , time is 5min;

[0143] (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent sensing modifier for expansion treatment, wherein the expansion rate is 80%, the temperature is 45° C., and the mass concentration of the temperature intelligent sensing modifier in the atomized environment is 90%;

[0144] (4) subjecting the veneer treated in step (3) to vacuum drying at a temperature of 40° C. to obtain modified veneer;

[0145] (5) A layer of PUR hot melt adhesive is coated on the surface of the substrate, and then it is pressed with the modified veneer to form a graded intelligent induction wooden floor; the graded intelligent induction wooden floor is immersed in a silicone waterproofing agent for 10 minutes, and alumina wear-resistant particles are deposited on the surface of the graded intelligent induction wooden floor by a magnetron sputtering method to construct a hydrophobic wear-resistant layer. Specifically, the sputtering power is 100 W, the sputtering pressure is 1.8 MPa, and the sputtering time is 100 minutes in an argon atmosphere. Finally, freeze-drying is performed to obtain a finished product.

[0146] The substrate is a modified substrate, which is prepared by the following method: placing the substrate in a closed impregnation treatment tank, evacuating the tank to a vacuum degree of -0.095 MPa, and maintaining the vacuum for 30 minutes, introducing a pre-configured modified isocyanate solution under vacuum, and performing pressurized impregnation treatment on the substrate, with an impregnation pressure of 3 MPa and an impregnation time of 4 hours, wherein the modified isocyanate solution is discharged after depressurization every 60 minutes, and then re-pressurized to obtain the modified substrate; the substrate adopts a five-layer solid wood composite substrate;

[0147] The modified isocyanate solution includes 150g of phase change energy storage microcapsules, 450ml of wet strength agent, 800ml of sodium silicate and 1300ml of modified isocyanate;

[0148] The mass concentration of the wet strength agent is 20%, and the mass concentration of the sodium silicate is 40%.

[0149] Example 3

[0150] A. Preparation of modified solution:

[0151] Take 48g of silver mercury iodide powder and 240ml of isopropanol and ultrasonically disperse them at 55°C for 45min, add 150ml of tetraethyl orthosilicate, 110ml of 3-aminopropyltriethoxysilane, 60ml of ammonia water and 1435ml of deionized water, stir at 70°C for 2h, add 315ml of 1% concentration NFC, and ultrasonicate at 75°C for 30min to obtain A modified solution.

[0152] Preparation of temperature intelligent sensing modifier:

[0153] 1200 ml of modified solution A and 100 g of crystal violet lactone were mixed, and the mixture was stirred for 60 minutes to obtain a temperature intelligent sensing modifier.

[0154] A preparation method of graded intelligent induction wood floor:

[0155] (1) 2.2 mm veneer was selected and placed in a supercritical device. The supercritical fluid was carbon dioxide and benzene-ethanol solution was used as an entrainer. The veneer was subjected to supercritical pretreatment. The supercritical temperature was set to 40 ° C, the pressure was set to 22 MPa, the time was set to 60 min, and the flow rate was set to 22 L / h;

[0156] (2) The veneer treated in step (1) is placed in a press for 120°C high-temperature steam softening and compression treatment, with a compression rate of 60% and a hot pressing pressure of 2 MPa / m 2 , time is 5min;

[0157] (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent sensing modifier for expansion treatment, wherein the expansion rate is 85%, the temperature is 55° C., and the mass concentration of the temperature intelligent sensing modifier in the atomized environment is 90%;

[0158] (4) subjecting the veneer treated in step (3) to vacuum drying at a temperature of 40° C. to obtain modified veneer;

[0159] (5) A layer of PUR hot melt adhesive is coated on the surface of the substrate, and then it is pressed with the modified veneer to form a graded intelligent induction wooden floor; the graded intelligent induction wooden floor is immersed in a silicone waterproofing agent for 10 minutes, and alumina wear-resistant particles are deposited on the surface of the graded intelligent induction wooden floor by a magnetron sputtering method to construct a hydrophobic wear-resistant layer. Specifically, the sputtering power is 100 W, the sputtering pressure is 2.2 MPa, and the sputtering time is 80 minutes in an argon atmosphere. Finally, freeze-drying is performed to obtain a finished product.

[0160] The substrate is a modified substrate, which is prepared by the following method: placing the substrate in a closed impregnation treatment tank, evacuating the tank to a vacuum degree of -0.095 MPa, and maintaining the vacuum for 30 minutes, introducing a pre-configured modified isocyanate solution under vacuum, and performing pressurized impregnation treatment on the substrate, with an impregnation pressure of 3.5 MPa and an impregnation time of 4 hours, wherein the modified isocyanate solution is discharged after depressurization every 60 minutes, and then re-pressurized to obtain the modified substrate; the substrate adopts a five-layer solid wood composite substrate;

[0161] The modified isocyanate solution includes 200g of phase change energy storage microcapsules, 550ml of wet strength agent, 950ml of sodium silicate and 1400ml of modified isocyanate;

[0162] The mass concentration of the wet strength agent is 20%, and the mass concentration of the sodium silicate is 40%.

[0163] Example 4

[0164] A. Preparation of modified solution:

[0165] Take 44 g of silver mercury iodide powder and 190 ml of isopropanol and ultrasonically disperse them at 55 ° C for 45 min, add 175 ml of tetraethyl orthosilicate, 100 ml of 3-aminopropyltriethoxysilane, 60 ml of ammonia water and 1500 ml of deionized water, stir at 70 ° C for 2 h, add 280 ml of 1% concentration NFC, and ultrasonicate at 75 ° C for 30 min to obtain A modified solution.

[0166] Preparation of B modified solution:

[0167] In an argon protective environment, 585 ml of MDI250, 156 g of PEG800 and 780 ml of toluene solution were added at 45 ° C, the temperature was raised to 75 ° C and stirred for 35 min, 43 g of 2,2-dihydroxymethylpropionic acid, 220 ml of modified crystal violet lactone and 15 g of dibutyltin dilaurate were slowly added dropwise, and the reaction was carried out at 80 ° C for 2 h, 57 g of caprolactam was added, the temperature was raised to 85 ° C and maintained for 30 min, the temperature was lowered to 45 ° C and 20 ml of triethylamine was added and maintained for 20 min, 1220 ml of deionized water and 30 ml of OP-10 emulsifier were added for emulsification and dispersion, and B modified liquid was obtained.

[0168] The modified crystal violet lactone is prepared by the following method: 80 g of crystal violet lactone is dissolved in 200 ml of isopropanol, ultrasonically treated for 15 min, 40 ml of hydrogen bromide is added to react at room temperature for 30 min, then 70 ml of 30% mass concentration of sodium hydroxide is added for hydrolysis, and deionized water is used for washing 3 times to obtain the modified crystal violet lactone.

[0169] Preparation of temperature intelligent sensing modifier:

[0170] 2300 ml of modified solution A was mixed with 1800 ml of modified solution B, and 33 ml of defoamer DE-H033 was added, and the mixture was stirred at 700 rpm for 60 min at 50° C. to obtain a temperature intelligent sensing modifier.

[0171] A preparation method of graded intelligent induction wood floor:

[0172] (1) 2.2 mm veneer was selected and placed in a supercritical device. The supercritical fluid was carbon dioxide and benzene-ethanol solution was used as an entrainer. The veneer was subjected to supercritical pretreatment. The supercritical temperature was set to 38 ° C, the pressure was set to 20 MPa, the time was set to 60 min, and the flow rate was set to 25 L / h;

[0173] (2) The veneer treated in step (1) is placed in a press for 110°C high-temperature steam softening and compression treatment, with a compression rate of 65% and a hot pressing pressure of 2 MPa / m 2 , time is 5min;

[0174] (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent sensing modifier for expansion treatment, wherein the expansion rate is 85%, the temperature is 60° C., and the mass concentration of the temperature intelligent sensing modifier in the atomized environment is 90%;

[0175] (4) subjecting the veneer treated in step (3) to vacuum drying at a temperature of 40° C. to obtain modified veneer;

[0176] (5) A layer of PUR hot melt adhesive is coated on the surface of the substrate, and then it is pressed with the modified veneer to form a graded intelligent induction wooden floor; the graded intelligent induction wooden floor is immersed in a silicone waterproofing agent for 10 minutes, and alumina wear-resistant particles are deposited on the surface of the graded intelligent induction wooden floor by a magnetron sputtering method to construct a hydrophobic wear-resistant layer. Specifically, the sputtering power is 100 W, the sputtering pressure is 2.2 MPa, and the sputtering time is 80 minutes in an argon atmosphere. Finally, freeze-drying is performed to obtain a finished product.

[0177] The substrate is a modified substrate, which is prepared by the following method: placing the substrate in a closed impregnation treatment tank, evacuating the tank to a vacuum degree of -0.095 MPa, and maintaining the vacuum for 30 minutes, introducing a pre-configured modified isocyanate solution under vacuum, and performing pressurized impregnation treatment on the substrate, with an impregnation pressure of 3 MPa and an impregnation time of 4 hours, wherein the modified isocyanate solution is discharged after depressurization every 60 minutes, and then re-pressurized to obtain the modified substrate; the substrate adopts a five-layer solid wood composite substrate;

[0178] The modified isocyanate solution includes 200g of phase change energy storage microcapsules, 780ml of wet strength agent, 950ml of sodium silicate and 1450ml of modified isocyanate;

[0179] The mass concentration of the wet strength agent is 20%, and the mass concentration of the sodium silicate is 40%.

[0180] Example 5

[0181] A. Preparation of modified solution:

[0182] Take 36 g of silver mercury iodide powder and 180 ml of isopropanol and ultrasonically disperse them at 55 ° C for 45 min, add 150 ml of tetraethyl orthosilicate, 120 ml of 3-aminopropyltriethoxysilane, 60 ml of ammonia water and 1500 ml of deionized water, stir at 70 ° C for 2 h, add 300 ml of 1% concentration NFC, and ultrasonicate at 75 ° C for 30 min to obtain A modified solution.

[0183] Preparation of B modified solution:

[0184] In an argon protective environment, add 600 ml of MDI250, 150 g of PEG800 and 800 ml of toluene solution at 45 ° C, heat to 75 ° C and stir for 35 minutes, slowly add 40 g of 2,2-dihydroxymethylpropionic acid, 220 ml of modified crystal violet lactone and 15 g of dibutyltin dilaurate, react at 80 ° C for 2 hours, add 60 g of caprolactam, heat to 85 ° C and keep for 30 minutes, cool to 45 ° C and add 20 ml of triethylamine and keep for 20 minutes, add 1230 ml of deionized water and 33 ml of OP-10 emulsifier for emulsification and dispersion, and obtain B modified liquid.

[0185] The modified crystal violet lactone is prepared by the following method: 80 g of crystal violet lactone is dissolved in 200 ml of isopropanol, ultrasonically treated for 15 min, 40 ml of hydrogen bromide is added to react at room temperature for 30 min, then 70 ml of 30% mass concentration of sodium hydroxide is added for hydrolysis, and deionized water is used for washing 3 times to obtain the modified crystal violet lactone.

[0186] Preparation of temperature intelligent sensing modifier:

[0187] 2280 ml of modified solution A was mixed with 1520 ml of modified solution B, and 31 ml of defoamer DE-H033 was added, and the mixture was stirred at 700 rpm for 60 min at 50° C. to obtain a temperature intelligent sensing modifier.

[0188] A preparation method of graded intelligent induction wood floor:

[0189] (1) Selecting 1.2 mm veneer, placing it in a supercritical device, using carbon dioxide as the supercritical fluid, using benzene-ethanol solution as an entrainer, performing a first supercritical pretreatment on the veneer, setting the supercritical temperature to 35° C., the pressure to 18 MPa, the time to 30 min, and the flow rate to 20 L / h; after the first supercritical pretreatment, adding maleic anhydride and dissolving it in the carbon dioxide fluid to obtain a mixed solution, and performing a second supercritical pretreatment on the veneer, wherein the amount of maleic anhydride added is 50% of the mass of the mixed solution, setting the supercritical temperature to 55° C., the pressure to 10 MPa, the time to 60 min, and the flow rate to 18 L / h;

[0190] (2) The veneer treated in step (1) is placed in a press for 100°C high-temperature steam softening and compression treatment, with a compression rate of 50% and a hot pressing pressure of 2 MPa / m 2 , time is 5min;

[0191] (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent sensing modifier for expansion treatment, wherein the expansion rate is 75%, the temperature is 45° C., and the mass concentration of the temperature intelligent sensing modifier in the atomized environment is 80%;

[0192] (4) subjecting the veneer treated in step (3) to vacuum drying at a temperature of 40° C. to obtain modified veneer;

[0193] (5) A layer of PUR hot melt adhesive is coated on the surface of the substrate, and then it is pressed with the modified veneer to form a graded intelligent induction wooden floor; the graded intelligent induction wooden floor is immersed in a silicone waterproofing agent for 10 minutes, and alumina wear-resistant particles are deposited on the surface of the graded intelligent induction wooden floor by a magnetron sputtering method to construct a hydrophobic wear-resistant layer. Specifically, the sputtering power is 100 W, the sputtering pressure is 2 MPa, and the sputtering time is 80 minutes in an argon atmosphere. Finally, freeze-drying is performed to obtain a finished product.

[0194] The substrate is a modified substrate, which is prepared by the following method: placing the substrate in a closed impregnation treatment tank, evacuating the tank to a vacuum degree of -0.095 MPa, and maintaining the vacuum for 30 minutes, introducing a pre-configured modified isocyanate solution under vacuum, and performing pressurized impregnation treatment on the substrate, with an impregnation pressure of 3 MPa and an impregnation time of 3 hours, wherein the modified isocyanate solution is discharged after depressurization every 60 minutes, and then re-pressurized to obtain the modified substrate; the substrate adopts a five-layer solid wood composite substrate;

[0195] The modified isocyanate solution includes 240g of phase change energy storage microcapsules, 510ml of wet strength agent, 690ml of sodium silicate and 1440ml of modified isocyanate;

[0196] The mass concentration of the wet strength agent is 20%, and the mass concentration of the sodium silicate is 40%.

[0197] Example 6

[0198] A. Preparation of modified solution:

[0199] Take 40g of silver mercury iodide powder and 140ml of isopropanol, ultrasonically disperse them at 60°C for 45min, add 100ml of tetraethyl orthosilicate, 80ml of 3-aminopropyltriethoxysilane, 60ml of ammonia water and 1400ml of deionized water, stir at 70°C for 2h, add 300ml of 1% concentration NFC, and ultrasonicate at 75°C for 30min to obtain A modified solution.

[0200] Preparation of B modified solution:

[0201] In an argon protective environment, 420 ml of MDI250, 126 g of PEG800 and 560 ml of toluene solution were added at 50 ° C, the temperature was raised to 80 ° C and stirred for 40 min, 42 g of 2,2-dihydroxymethylpropionic acid, 175 ml of modified crystal violet lactone and 14 g of dibutyltin dilaurate were slowly added dropwise, and the reaction was carried out at 80 ° C for 2.5 h, 56 g of caprolactam was added, the temperature was raised to 85 ° C and maintained for 30 min, the temperature was lowered to 47 ° C and 21 ml of triethylamine was added and maintained for 20 min, 882 ml of deionized water and 24 ml of OP-10 emulsifier were added for emulsification and dispersion, and B modified liquid was obtained.

[0202] The modified crystal violet lactone was prepared by the following method: 80 g of crystal violet lactone was dissolved in 220 ml of isopropanol, ultrasonically treated for 20 min, 40 ml of hydrogen bromide was added and reacted at room temperature for 30 min, then 78 ml of 30% mass concentration of sodium hydroxide was added for hydrolysis, and deionized water was used for washing 4 times to obtain the modified crystal violet lactone.

[0203] Preparation of temperature intelligent sensing modifier:

[0204] 1900 ml of modified solution A was mixed with 1900 ml of modified solution B, and 31 ml of defoamer DE-H033 was added, and the mixture was stirred at 700 rpm for 60 min at 50° C. to obtain a temperature intelligent sensing modifier.

[0205] A preparation method of graded intelligent induction wood floor:

[0206] (1) selecting 2 mm veneer and placing it in a supercritical device, wherein the supercritical fluid is carbon dioxide and a benzene-ethanol solution is used as an entrainer, and the veneer is subjected to a first supercritical pretreatment, wherein the supercritical temperature is set to 40° C., the pressure is set to 20 MPa, the time is set to 60 min, and the flow rate is set to 20 L / h; after the first supercritical pretreatment, maleic anhydride is added and dissolved in the carbon dioxide fluid to obtain a mixed solution, and the veneer is subjected to a second supercritical pretreatment, wherein the amount of maleic anhydride added is 60% of the mass of the mixed solution, and the supercritical temperature is set to 60° C., the pressure is set to 10 MPa, the time is set to 90 min, and the flow rate is set to 20 L / h;

[0207] (2) The veneer treated in step (1) is placed in a press for 120°C high-temperature steam softening and compression treatment, with a compression rate of 60% and a hot pressing pressure of 2 MPa / m 2 , time is 10min;

[0208] (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent sensing modifier for expansion treatment, wherein the expansion rate is 85%, the temperature is 60° C., and the mass concentration of the temperature intelligent sensing modifier in the atomized environment is 95%;

[0209] (4) subjecting the veneer treated in step (3) to vacuum drying at a temperature of 40° C. to obtain modified veneer;

[0210] (5) A layer of PUR hot melt adhesive is coated on the surface of the substrate, and then it is pressed with the modified veneer to form a graded intelligent induction wooden floor; the graded intelligent induction wooden floor is immersed in a silicone waterproofing agent for 10 minutes, and alumina wear-resistant particles are deposited on the surface of the graded intelligent induction wooden floor by a magnetron sputtering method to construct a hydrophobic wear-resistant layer. Specifically, the sputtering power is 100 W, the sputtering pressure is 2 MPa, and the sputtering time is 80 minutes in an argon atmosphere. Finally, freeze-drying is performed to obtain a finished product.

[0211] The substrate is a modified substrate, which is prepared by the following method: placing the substrate in a closed impregnation treatment tank, evacuating the tank to a vacuum degree of -0.095 MPa, and maintaining the vacuum for 30 minutes, introducing a pre-configured modified isocyanate solution under vacuum, and performing pressurized impregnation treatment on the substrate, with an impregnation pressure of 3.5 MPa and an impregnation time of 4 hours, wherein the modified isocyanate solution is discharged after depressurization every 60 minutes, and then re-pressurized to obtain the modified substrate; the substrate adopts a five-layer solid wood composite substrate;

[0212] The modified isocyanate solution includes 90g of phase change energy storage microcapsules, 60ml of wet strength agent, 1050ml of sodium silicate and 1290ml of modified isocyanate;

[0213] The mass concentration of the wet strength agent is 20%, and the mass concentration of the sodium silicate is 40%.

[0214] Example 7

[0215] A. Preparation of modified solution:

[0216] Take 52.5 g of silver mercury iodide powder and 120 ml of isopropanol, ultrasonically disperse them at 65 ° C for 60 min, add 90 ml of tetraethyl orthosilicate, 67.5 ml of 3-aminopropyltriethoxysilane, 45 ml of ammonia water and 1200 ml of deionized water, stir at 70 ° C for 2 h, add 370 ml of 1% concentration NFC, and ultrasonicate at 75 ° C for 30 min to obtain A modified solution.

[0217] Preparation of B modified solution:

[0218] In an argon protective environment, add 560 ml of MDI250, 160 g of PEG800 and 680 ml of toluene solution at 50 ° C, heat to 80 ° C and stir for 40 min, slowly add 64 g of 2,2-dihydroxymethylpropionic acid, 240 ml of modified crystal violet lactone and 20 g of dibutyltin dilaurate, react at 80 ° C for 2.5 h, add 80 g of caprolactam, heat to 85 ° C and keep for 30 min, cool to 47 ° C and add 40 ml of triethylamine and keep for 20 min, add 1140 ml of deionized water and 61 ml of OP-10 emulsifier for emulsification and dispersion, and obtain B modified liquid.

[0219] The modified crystal violet lactone is prepared by the following method: 80 g of crystal violet lactone is dissolved in 200 ml of isopropanol, ultrasonically treated for 20 min, 72 ml of hydrogen bromide is added to react at room temperature for 30 min, then 82 ml of 30% mass concentration of sodium hydroxide is added for hydrolysis, and deionized water is used for washing 4 times to obtain the modified crystal violet lactone.

[0220] Preparation of temperature intelligent sensing modifier:

[0221] 1330 ml of modified solution A was mixed with 2470 ml of modified solution B, and 38 ml of defoamer DE-H033 was added, and the mixture was stirred at 700 rpm for 60 min at 60° C. to obtain a temperature intelligent sensing modifier.

[0222] A preparation method of graded intelligent induction wood floor:

[0223] (1) Selecting 2.5 mm veneer, placing it in a supercritical device, using carbon dioxide as the supercritical fluid, using benzene-ethanol solution as an entrainer, and performing a first supercritical pretreatment on the veneer, setting the supercritical temperature to 40° C., the pressure to 25 MPa, the time to 60 min, and the flow rate to 30 L / h; after the first supercritical pretreatment, adding maleic anhydride and dissolving it in the carbon dioxide fluid to obtain a mixed solution, and performing a second supercritical pretreatment on the veneer, wherein the amount of maleic anhydride added is 70% of the mass of the mixed solution, and setting the supercritical temperature to 60° C., the pressure to 11 MPa, the time to 120 min, and the flow rate to 25 L / h;

[0224] (2) The veneer treated in step (1) is placed in a press for 120°C high-temperature steam softening and compression treatment, with a compression rate of 70% and a hot pressing pressure of 2.5 MPa / m 2 , time is 15min;

[0225] (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent sensing modifier for expansion treatment, wherein the expansion rate is 85%, the temperature is 55° C., and the mass concentration of the temperature intelligent sensing modifier in the atomized environment is 95%;

[0226] (4) subjecting the veneer treated in step (3) to vacuum drying at a temperature of 40° C. to obtain modified veneer;

[0227] (5) A layer of PUR hot melt adhesive is coated on the surface of the substrate, and then it is pressed with the modified veneer to form a graded intelligent induction wooden floor; the graded intelligent induction wooden floor is immersed in a silicone waterproofing agent for 10 minutes, and alumina wear-resistant particles are deposited on the surface of the graded intelligent induction wooden floor by a magnetron sputtering method to construct a hydrophobic wear-resistant layer. Specifically, the sputtering power is 100 W, the sputtering pressure is 2 MPa, and the sputtering time is 80 minutes in an argon atmosphere. Finally, freeze-drying is performed to obtain a finished product.

[0228] The substrate is a modified substrate, which is prepared by the following method: placing the substrate in a closed impregnation treatment tank, evacuating the tank to a vacuum degree of -0.095 MPa, and maintaining the vacuum for 30 minutes, introducing a pre-configured modified isocyanate solution under vacuum, and performing pressurized impregnation treatment on the substrate, with an impregnation pressure of 3.5 MPa and an impregnation time of 5 hours, wherein the modified isocyanate solution is discharged after depressurization every 60 minutes, and then re-pressurized to obtain the modified substrate; the substrate adopts a five-layer solid wood composite substrate;

[0229] The modified isocyanate solution includes 210 g of phase change energy storage microcapsules, 900 ml of wet strength agent, 780 ml of sodium silicate and 1260 ml of modified isocyanate;

[0230] The mass concentration of the wet strength agent is 20%, and the mass concentration of the sodium silicate is 40%.

[0231] The graded intelligent induction wood floorings prepared in Examples 1-7 were tested, and the test results were as follows:

[0232] 1. Determination of the first color change temperature: Place the graded intelligent induction wooden floor in an oven. As the temperature rises from <30°C, the color of the wooden floor begins to change from green to purple. The temperature at which the color of the wooden floor stabilizes at purple is the first color change temperature.

[0233] 2. Determination of the second color change temperature: Place the graded intelligent induction wooden floor in an oven. As the temperature rises from 40°C, the color of the wooden floor changes from purple to red. The temperature at which the color of the wooden floor stabilizes at red is the second color change temperature.

[0234] 3. Determination of color change time: Place the graded intelligent induction wooden floor in an oven. As the temperature rises from <30°C, the time from when the color of the wooden floor changes from green to purple to when the color stabilizes at purple is the color change time.

[0235] 4. Color difference value determination: Use a colorimeter to detect the color difference value of the graded intelligent induction wooden floor. The color difference value = the color difference value after color change - the color difference value before color change;

[0236] 5. Determination of phase change enthalpy and phase change temperature: Determine according to "GB 19466.3-2004 Plastics Differential Scanning Calorimetry (DSC) Part 3: Determination of Melting and Crystallization Temperature and Enthalpy";

[0237] 6. Determination of contact angle: Determine according to GB / T 30447-2013 Contact angle measurement method of nanofilm;

[0238] 7. Determination of surface wear resistance: Determine according to GB 18103-2013 Solid Wood Composite Flooring.

[0239] The above test results are shown in Table 1.

[0240] Table 1 Test results of graded intelligent induction wood floorings prepared in Examples 1-7

[0241]

[0242] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A method for preparing a graded intelligent induction wooden floor, characterized in that: The following steps are involved: (1) supercritical pretreatment of veneer; (2) subjecting the veneer treated in step (1) to high temperature steam softening and compression treatment; (3) placing the veneer treated in step (2) in an atomized environment of a temperature intelligent sensing modifier for expansion treatment; (4) vacuum drying the veneer treated in step (3) to obtain modified veneer; (5) coating a layer of adhesive on the surface of the substrate, and then pressing and molding with the modified veneer to obtain a graded intelligent induction wood floor; Wherein, the temperature intelligent sensing modifier comprises a temperature-sensitive color-changing material and a modified crystal violet lactone; Calculated by volume, the temperature intelligent sensing modifier includes 25-85 parts of A modified solution, 18-75 parts of B modified solution and 0.5-1.2 parts of defoaming agent; The raw materials for preparing the modified solution A include 0.8-4 parts by mass of a temperature-sensitive color-changing material, 5-9 parts by volume of a first solvent, 4-7 parts by volume of a silane crosslinking agent, 3-6 parts by volume of a silane coupling agent, 1-5 parts by volume of ammonia water, 40-80 parts by volume of deionized water, and 10-30 parts by volume of nanofibrillated cellulose; The raw materials for preparing the B modified solution include 50-80 parts by volume of isocyanate, 10-25 parts by volume of polyethylene glycol, 70-90 parts by volume of a second solvent, 4-8 parts by volume of a chain extender, 20-40 parts by volume of a modified crystal violet lactone, 1-2.8 parts by volume of a catalyst, 5.4-10 parts by volume of a capping agent, 1-5 parts by volume of a salt-forming agent, 70-85 parts by volume of deionized water and 1-5 parts by volume of an emulsifier; The temperature-sensitive color-changing material is one or more of silver mercury iodide and copper mercury iodide; The preparation method of the modified solution A is as follows: 0.8-4 parts by mass of a thermochromic material and 5-9 parts by volume of a first solvent are ultrasonically dispersed at a temperature of 55-65° C. for 30-60 minutes, and then 4-7 parts by volume of a silane crosslinking agent, 3-6 parts by volume of a silane coupling agent, 1-5 parts by volume of ammonia water and 40-80 parts by volume of deionized water are added, and stirred at 70° C. for 1.5-3 hours, and then 10-30 parts by volume of nanofibrillated cellulose with a mass concentration of 0.8%-1.5% is added, and ultrasonicated at 70-80° C. for 30 minutes to obtain the modified solution A; Wherein, the first solvent is one or more of isopropanol, toluene, methanol, ethanol, dichloromethane, and acetone; The silane crosslinking agent is one or more of ethyl orthosilicate, methyltriacetoxysilane, methyltrimethoxysilane, and methyltributylidene oxime silane; The silane coupling agent is one or more of 3-aminopropyltriethoxysilane, tributylaminomethylsilane, γ-aminoethylaminopropyltrimethoxysilane, and N-aminoethyl-3-aminopropylmethyldimethoxysilane; The preparation method of the B modified solution comprises: adding 50-80 parts by volume of isocyanate, 10-25 parts by volume of polyethylene glycol and 70-90 parts by volume of a second solvent at 45-60° C. in an argon protective environment, and mixing; then heating to 70-80° C. and stirring for 30-45 minutes, slowly dropping 4-8 parts by volume of a chain extender, 20-40 parts by volume of a modified crystal violet lactone and 1-2.8 parts by volume of a catalyst, and reacting at 75° C.-80° C. for 2-3 hours; then adding 5.4-10 parts by volume of a capping agent, heating to 85° C. and maintaining for 30 minutes; cooling to 40-60° C., adding 1-5 parts by volume of a salt-forming agent, maintaining for 15-40 minutes, adding 70-85 parts by volume of deionized water and 1-5 parts by volume of an emulsifier for emulsification and dispersion, and obtaining the B modified solution; The isocyanate is one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate; The second solvent is one or more of benzene, toluene, carbon tetrachloride, acetone, ethyl acetate, dimethyl sulfoxide, chloroform, N,N-dimethylformamide and N,N-dimethylacetamide; The chain extender is one or more of 2,2-dimethylol propionic acid, dihydroxy half ester, sodium ethylenediaminoethanesulfonate, diethylenetriamine or methyldiethanolamine; The catalyst is one or more of dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, stannous octoate, dimethyltin dineodecanoate, and dibutyltin bis(β-diketonate); The end-capping agent is caprolactam; The salt-forming agent is one or more of triethylamine, hydrochloric acid, acetic acid, and propylene oxide; The preparation method of the temperature intelligent sensing modifier: Calculated by volume, 25-85 parts of modified solution A and 18-75 parts of modified solution B are mixed, and then 0.5-1.2 parts of defoaming agent are added, and stirred at 450-1000 rpm for 30-90 minutes at 45-70°C to obtain a temperature intelligent sensing modifier; Step (1) comprises: (11) The supercritical fluid is carbon dioxide, and a benzene-ethanol solution is used as an entrainer to perform a first supercritical pretreatment on the veneer; wherein the supercritical temperature is 35-45° C., the pressure is 10-30 MPa, the time is 30-100 min, and the flow rate is 10-40 L / h; (12) After the first supercritical pretreatment, maleic anhydride is added and dissolved in the carbon dioxide fluid to obtain a mixed solution, and the veneer is subjected to a second supercritical pretreatment; wherein the supercritical temperature is 50-65° C., the pressure is 8-15 MPa, the time is 60-120 min, and the flow rate is 10-30 L / h; The amount of maleic anhydride added is 30-75% of the mass of the mixed solution.

2. The method for preparing the graded intelligent induction wooden floor according to claim 1, characterized in that: The preparation method of the modified crystal violet lactone is: 1.5-3 parts by mass of crystal violet lactone is dissolved in 3-10 parts by volume of a third solvent, subjected to ultrasonic treatment for 10-30 minutes, and 1-5 parts by volume of hydrogen bromide is added and reacted at room temperature for 20-80 minutes to obtain a mixed solution; Adding sodium hydroxide with a mass concentration of 20-40% to the mixed solution for hydrolysis, and then washing with deionized water for 3-5 times to obtain modified crystal violet lactone; Wherein, the amount of sodium hydroxide added is 20-50% of the volume of the mixed solution; The third solvent is one or more of isopropanol, toluene, methanol, ethanol, dichloromethane, and acetone.

3. The method for preparing the graded intelligent induction wooden floor according to claim 1, characterized in that: The thickness of the veneer is 1.0-3.0 mm; The temperature of step (2) is 100-120°C, the compression rate is set to 50-70%, and the unit hot pressing pressure is 1.5-3MPa / m 2 , hot pressing time is 5-20min; Step (3) setting the expansion rate to 60-90%, the temperature to 40-65° C., and the mass concentration of the temperature intelligent sensing modifier in the atomization environment to 80-100%; The temperature of step (4) is 35-45°C.

4. The method for preparing the graded intelligent induction wooden floor according to claim 1, characterized in that: The substrate is a modified substrate; The modified substrate is prepared by the following method: The substrate is placed in a sealed impregnation tank, and the vacuum is drawn to a vacuum degree of -(0.090-0.097) MPa for 25-35 minutes. The pre-configured modified isocyanate solution is introduced under vacuum, and the substrate is subjected to pressurized impregnation treatment, with an impregnation pressure of 2.5-4 MPa and an impregnation time of 3-5 hours. The modified isocyanate solution is discharged after the pressure is released every 60 minutes, and then the pressure is re-applied to obtain a modified substrate; The modified isocyanate solution comprises 2-10 parts by mass of phase change energy storage microcapsules, 15-35 parts by volume of a wet strength agent, 20-50 parts by volume of sodium silicate and 40-68 parts by volume of modified isocyanate; The mass concentration of the wet strength agent is 18-20%, and the mass concentration of the sodium silicate is 35-45%; The substrate is also provided with a high thermal conductivity film; The graded intelligent induction wooden floor is also provided with a waterproof layer and a wear-resistant layer.

5. A hierarchical intelligent induction wooden floor, characterized in that: The wood floor is prepared by the method for preparing the graded intelligent induction wood floor according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Temperature-sensitive color-changing floor and preparation method thereof

    CN112795295A

  • Dipping modification treatment method of solid wood floor for floor heating

    CN114083631A

  • Color-changeable carbon fiber heating floorboard

    CN204174873U

  • A plank that discolours for bathroom

    CN204728632U

  • Woody floor material

    JP2013024001A