Screen printing ink
Through the combination of surface-modified silver nanoparticles and low-boiling terpene solvents, the problems of insufficient viscosity and solvent volatility of screen printing ink are solved, high-precision drawing and continuous printing are achieved, and electronic components with high adhesion and conductivity are obtained. .
Patent Information
- Application Number
- CN202211391752.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-04-04
- Filing Date
- 2017-03-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2037-03-30
AI Technical Summary
Existing screen printing inks have problems with insufficient viscosity and solvent volatility in the high-precision drawing of thin lines and continuous printing, making it difficult to form electronic components with high adhesion and conductivity.
The combination of surface-modified silver nanoparticles and low-boiling terpene solvents is used to prepare inks with specific viscosity, inhibit solvent volatility and prevent mesh clogging, and electronic components are manufactured by screen printing.
High-precision drawing of thin lines and continuous printing are achieved, and excellent substrate adhesion and conductive sintered bodies are obtained, which are suitable for the manufacturing of electronic components on plastic substrates.
Smart Images

Figure QLYQS_1 
Figure BDA0003931249800000031 
Figure BDA0003931249800000131
Abstract
Description
[0001] The present application is a divisional application of an application with a filing date of March 30, 2017, an application number of 201780021027.0, and an invention name of “Ink for Screen Printing”. Technical Field
[0002] The present invention relates to an ink for use in manufacturing electronic components using a screen printing method. This application claims priority to Japanese Patent Application No. 2016-075037 filed in Japan on April 4, 2016, and the contents thereof are incorporated herein by reference. Background Art
[0003] Since silver nanoparticles can be sintered at low temperatures, they can be used to form electronic components such as electrodes or wiring on plastic substrates. However, silver nanoparticles have the problem of being easily agglomerated. Patent Document 1 discloses that by coating the surface of silver nanoparticles with an amine-containing protective agent, good dispersion stability can be obtained in a solvent, and the ink obtained by dispersing the silver nanoparticles in a solvent containing alicyclic hydrocarbons or alcohols is suitable for inkjet printing.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2014 / 021270 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] However, since the viscosity of the ink is too low for screen printing, it is easy to blur and it is difficult to draw fine lines with high precision. In addition, in the case of screen printing, there is a problem that the ink remains in the screen after printing, but when the residual ink contains a solvent such as a highly volatile alcohol, the ink becomes thicker or dries and solidifies due to the volatilization of the solvent, causing the mesh to be clogged, making continuous printing difficult.
[0009] Therefore, an object of the present invention is to provide an ink for use in manufacturing electronic parts by screen printing, the ink being capable of drawing fine lines with high precision by screen printing and being capable of continuously performing screen printing.
[0010] Another object of the present invention is to provide an ink for use in manufacturing electronic components using a screen printing method, wherein the ink can draw fine lines with high precision by screen printing, can perform screen printing continuously, and can form electronic components having excellent substrate adhesion.
[0011] Another object of the present invention is to provide a method for manufacturing electronic devices using the ink.
[0012] Another object of the present invention is to provide an electronic device including a sintered body of the ink.
[0013] Technical means to solve technical problems
[0014] As a result of intensive research to solve the above problems, the inventors found that an ink with a specific viscosity obtained by dispersing silver nanoparticles having a structure in which the surface is coated with an amine-containing protective agent in a specific solvent, that is, a solvent containing at least a terpene solvent and having a boiling point of less than 130° C. and having a content of 20% by weight or less, can be used to draw high-precision fine lines by screen printing, and the volatility of the ink at the printing temperature is extremely low, so that the clogging of the mesh of the screen is suppressed, and continuous printing can be performed. Based on these findings, the present invention was completed.
[0015] It should be noted that, in this specification, "nanoparticles" refer to particles whose primary particle size (average primary particle size) is less than 1000 nm. In addition, the particle size is obtained by observation with a scanning electron microscope (SEM). In addition, the boiling point in this specification refers to the value at normal pressure (760 mmHg).
[0016] That is, the present invention provides a screen printing ink comprising the following surface-modified silver nanoparticles (A) and the following solvent (B), wherein the viscosity of the screen printing ink (at 25° C. and a shear rate of 10 (1 / s)) is 60 Pa·s or more.
[0017] Surface-modified silver nanoparticles (A): The surface of the silver nanoparticles is coated with an amine-containing protective agent.
[0018] Solvent (B): contains at least a terpene solvent, and the content of the solvent having a boiling point lower than 130° C. is 20% by weight or less of the total amount of the solvent.
[0019] The present invention provides a screen printing ink, wherein the protective agent comprises, as amines, an aliphatic monoamine (1) having a total carbon number of 6 or more, and an aliphatic monoamine (2) having a total carbon number of 5 or less and / or an aliphatic diamine (3) having a total carbon number of 8 or less.
[0020] The present invention provides the screen printing ink, wherein the aliphatic monoamine (1) having a total carbon number of 6 or more is a monoamine having a linear alkyl group and a total carbon number of 6 to 18 and / or a monoamine having a branched alkyl group and a total carbon number of 6 to 16.
[0021] The present invention provides the screen printing ink, wherein the aliphatic monoamine (2) having a total carbon number of 5 or less is a monoamine having a straight-chain or branched alkyl group and a total carbon number of 2 to 5.
[0022] The present invention provides a screen printing ink, wherein the aliphatic diamine (3) having a total carbon number of 8 or less is represented by the following general formula (a-2):
[0023] [Chemical formula 1]
[0024]
[0025] (Where R 4 and R 5 are the same or different and are straight chain or branched chain alkyl groups, R 6 and R 7 is a hydrogen atom, R 8 is a straight chain or branched chain alkylene).
[0026] The present invention provides the screen printing ink, wherein the boiling point of the terpene solvent is 130° C. or higher, and the viscosity (at 20° C.) is 50 to 250 mPa·s.
[0027] The present invention provides the screen printing ink, wherein the solvent (B) further contains a glycol ether solvent having a boiling point of 130° C. or higher.
[0028] The present invention provides a screen printing ink, wherein the glycol ether solvent comprises a compound represented by the following formula (b):
[0029] R 11 -(OR 13 ) m -OR 12 (b)
[0030] (Where R 11 and R 12 are the same or different and represent an alkyl group or an acyl group, R 13 represents an alkylene group having 1 to 6 carbon atoms, and m represents an integer greater than 1).
[0031] The present invention provides the screen printing ink, which further contains a binder resin (C).
[0032] The present invention provides the above-mentioned screen printing ink, wherein the volume resistivity of a sintered body obtained by sintering at 120° C. for 30 minutes is 10 μΩcm or less.
[0033] The present invention provides a method for manufacturing an electronic device, comprising: a process of coating the screen printing ink on a substrate by screen printing; and a sintering process.
[0034] The present invention provides an electronic device having a sintered body of the screen printing ink on a substrate.
[0035] That is, the present invention relates to the following.
[0036] [1] A screen printing ink comprising the following surface-modified silver nanoparticles (A) and the following solvent (B), wherein the viscosity of the screen printing ink at 25°C and a shear rate of 10 (1 / s) is 60 Pa·s or more (preferably 70 Pa·s or more, more preferably 80 Pa·s or more, further preferably 90 Pa·s or more, further preferably 100 Pa·s or more, and particularly preferably 150 Pa·s or more. The upper limit of the viscosity is preferably 500 Pa·s, more preferably 450 Pa·s, further preferably 400 Pa·s, and most preferably 350 Pa·s).
[0037] Surface-modified silver nanoparticles (A): The surface of the silver nanoparticles is coated with an amine-containing protective agent.
[0038] Solvent (B): Contains at least a terpene solvent, and the content of the solvent having a boiling point below 130°C is 20 wt% or less (preferably 10 wt% or less, particularly preferably 5 wt% or less, and most preferably 1 wt% or less) of the total amount of the solvent.
[0039] [2] The screen printing ink according to [1], wherein the protective agent comprises, as amines, an aliphatic monoamine (1) having a total carbon number of 6 or more, and an aliphatic monoamine (2) having a total carbon number of 5 or less and / or an aliphatic diamine (3) having a total carbon number of 8 or less.
[0040] [3] The screen printing ink according to [2], wherein the aliphatic monoamine (1) having a total carbon number of 6 or more is a monoamine having a linear alkyl group and a total carbon number of 6 to 18 and / or a monoamine having a branched alkyl group and a total carbon number of 6 to 16.
[0041] [4] The screen printing ink according to [2], wherein the aliphatic monoamine (1) having a total carbon number of 6 or more is a primary amine having a linear or branched alkyl group.
[0042] [5] The screen printing ink according to [2], wherein the aliphatic monoamine (1) having a total carbon number of 6 or more is at least one compound selected from the group consisting of hexylamine, heptylamine, octylamine, nonylamine, decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, heptadecanamine, octadecylamine, isohexylamine, 2-ethylhexylamine, and tert-octylamine.
[0043] [6] The screen printing ink according to any one of [2] to [5], wherein the aliphatic monoamine (2) having a total carbon number of 5 or less is a primary amine having a linear or branched alkyl group and a total carbon number of 2 to 5 (preferably 4 to 5).
[0044] [7] The screen printing ink according to any one of [2] to [5], wherein the aliphatic monoamine (2) having a total carbon number of 5 or less is a primary amine having a straight-chain alkyl group and a total carbon number of 2 to 5 (preferably 4 to 5).
[0045] [8] The screen printing ink according to any one of [2] to [5], wherein the aliphatic monoamine (2) having a total carbon number of 5 or less is at least one compound selected from butylamine, isobutylamine, sec-butylamine, tert-butylamine, pentylamine, isopentylamine, and tert-pentylamine.
[0046] [9] The screen printing ink according to any one of [2] to [8], wherein the aliphatic monoamine (2) having a total carbon number of 5 or less is a primary amine having a linear or branched alkyl group and having a total carbon number of 2 to 5.
[0047]
[10] The screen printing ink according to any one of [2] to [9], wherein the aliphatic diamine (3) having a total carbon number of 8 or less is a diamine having a total carbon number of 1 to 8 represented by formula (a-2).
[0048]
[11] The screen printing ink according to any one of [2] to [9], wherein the aliphatic diamine (3) having a total carbon number of 8 or less is represented by formula (a-2), and wherein R 4 and R 5 are the same or different and are straight chain or branched chain alkyl groups, R 6 and R 7 is a hydrogen atom, R 8 It is a straight chain or branched chain alkylene group.
[0049]
[12] The screen printing ink according to any one of [2] to [9], wherein the aliphatic diamine (3) having a total carbon number of 8 or less is represented by formula (a-2), and wherein R 4 and R 5 is a straight chain alkyl group, R 6 and R 7 is a hydrogen atom, R 8 It is a straight chain alkylene group.
[0050]
[13] The screen printing ink according to any one of [2] to
[12] , wherein the content of monoamine (1) in the total amount of amines coating the surface of the silver nanoparticles in the surface-modified silver nanoparticles (A) is 5 to 65 mol% (the lower limit is preferably 10 mol%, particularly preferably 15 mol%. In addition, the upper limit is preferably 50 mol%, particularly preferably 40 mol%, and most preferably 35 mol%), and the content of monoamine (2) is 35 to 95 mol% (the lower limit is preferably 50 mol%, particularly preferably 60 mol%, and most preferably 65 mol%. In addition, the upper limit is preferably 90 mol%, and particularly preferably 85 mol%).
[0051]
[14] The screen printing ink according to any one of [2] to
[13] , wherein the total content of the monoamine (1), the monoamine (2), and the diamine (3) accounts for 60% by weight or more (preferably 80% by weight or more, particularly preferably 90% by weight or more) of the total amount of amines coating the surface of the silver nanoparticles in the surface-modified silver nanoparticles (A).
[0052]
[15] The screen printing ink according to any one of [1] to
[14] , wherein the terpene solvent has a boiling point of 130°C or higher and a viscosity (at 20°C) of 50 to 250 mPa·s.
[0053]
[16] The screen printing ink according to any one of [1] to
[15] , wherein the solvent (B) further contains a glycol ether solvent having a boiling point of 130° C. or higher.
[0054]
[17] The screen printing ink according to
[16] , wherein the glycol ether solvent contains a compound represented by the following general formula (b):
[0055] R 11 -(OR 13 ) m -OR 12 (b)
[0056] (Where R 11 and R 12 are the same or different and represent an alkyl group or an acyl group, R 13 represents an alkylene group having 1 to 6 carbon atoms, and m represents an integer greater than 1).
[0057]
[18] The screen printing ink according to
[16] , wherein the glycol ether solvent contains a compound represented by the following general formula (b'):
[0058] R 14 -(OR 15 ) n -OH (b')
[0059] (Where R 14 represents an alkyl or aryl group, R 15 represents an alkylene group having 1 to 6 carbon atoms, and n represents an integer greater than 1).
[0060]
[19] The screen printing ink according to
[16] , wherein the glycol ether solvent comprises a compound represented by the following formula (b) and / or a compound represented by the following formula (b'):
[0061] R 11 -(OR 13 ) m -OR 12 (b)
[0062] (Where R 11 and R 12 are the same or different and represent an alkyl group or an acyl group, R 13 represents an alkylene group having 1 to 6 carbon atoms, and m represents an integer greater than 1),
[0063] R 14 -(OR 15 ) n -OH (b')
[0064] (Where R 14 represents an alkyl or aryl group, R 15 represents an alkylene group having 1 to 6 carbon atoms, and n represents an integer greater than 1).
[0065]
[20] The screen printing ink according to
[17] or
[19] , wherein the compound represented by formula (b) has a boiling point of 130°C or higher (preferably 170°C or higher, particularly preferably 200°C or higher).
[0066]
[21] The screen printing ink according to
[17] or
[19] , wherein the compound represented by formula (b) has a boiling point of 130 to 300°C (preferably 170 to 300°C, particularly preferably 200 to 300°C).
[0067]
[22] The screen printing ink according to any one of
[17] ,
[19] to
[21] , wherein the compound represented by formula (b) is at least one compound selected from ethylene glycol diether, ethylene glycol ether acetate, and ethylene glycol diacetate.
[0068]
[23] The screen printing ink according to any one of
[17] ,
[19] to
[21] , wherein the compound represented by formula (b) is at least one compound selected from 1,3-butanediol diacetate, 1,4-butanediol diacetate, 1,6-hexanediol diacetate, diethylene glycol dibutyl ether, diethylene glycol methyl n-butyl ether, diethylene glycol n-butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, dipropylene glycol methyl isopentyl ether, dipropylene glycol methyl n-propyl ether, dipropylene glycol methyl n-butyl ether, dipropylene glycol methyl cyclopentyl ether, triethylene glycol dimethyl ether, triethylene glycol methyl n-butyl ether, tripropylene glycol methyl n-propyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0069]
[24] The screen printing ink according to any one of
[18] to
[23] , wherein the compound represented by formula (b') has a boiling point of 130° C. or higher (preferably 140° C. or higher).
[0070]
[25] The screen printing ink according to any one of
[18] to
[23] , wherein the compound represented by the general formula (b') has a boiling point of 130 to 310°C (preferably 130 to 250°C, particularly preferably 130 to 200°C, most preferably 130 to 180°C, and extremely preferably 140 to 180°C).
[0071]
[26] The screen printing ink according to any one of
[18] to
[25] , wherein the compound represented by the general formula (b') is selected from ethylene glycol monomethyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, ethylene glycol monotert-butyl ether, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, diethylene glycol monotert-butyl ether, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, diethylene glycol monotert-butyl ether, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, The invention relates to at least one compound selected from the group consisting of diethylene glycol monoisobutyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monopentyl ether, diethylene glycol monoisopentyl ether, diethylene glycol monohexyl ether, diethylene glycol mono-2-ethylhexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, triethylene glycol monomethyl ether, triethylene glycol monobutyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, and 3-methoxy-1-butanol.
[0072]
[27] An ink for screen printing according to any one of
[18] to
[25] , wherein the compound represented by the general formula (b') is at least one compound selected from ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, ethylene glycol monotert-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monopentyl ether, diethylene glycol monoisopentyl ether, diethylene glycol monohexyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, and 3-methoxy-1-butanol.
[0073]
[28] An ink for screen printing according to any one of
[18] to
[25] , wherein the compound represented by the general formula (b') is at least one compound selected from ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, ethylene glycol monotert-butyl ether, diethylene glycol monopentyl ether, diethylene glycol monoisopentyl ether, diethylene glycol monohexyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, and 3-methoxy-1-butanol.
[0074]
[29] The screen printing ink according to any one of [1] to
[28] , further comprising a binder resin (C).
[0075]
[30] The screen printing ink according to any one of [1] to
[29] , wherein the content of the surface-modified silver nanoparticles is 60 to 85 wt % (preferably 75 to 85 wt %) in the total amount of the screen printing ink (100 wt %).
[0076]
[31] The screen printing ink according to any one of [1] to
[29] , wherein the content of the surface-modified silver nanoparticles is 60 to 85 wt % (preferably 60 to 80 wt %, particularly preferably 60 to 75 wt %) in the total amount of the screen printing ink (100 wt %).
[0077]
[32] According to any one of [1] to
[31] , the content of terpene solvent in the total amount of screen printing ink (100 weight %) is 5 to 30 weight % (the lower limit is preferably 10 weight %, particularly preferably 14 weight %. The upper limit is preferably 25 weight %, particularly preferably 18 weight %).
[0078]
[33] According to any one of
[17] ,
[19] to
[32] , the content of the compound represented by the general formula (b) in the total amount of the screen printing ink (100 weight %) is 0.5 to 5 weight % (the lower limit is preferably 1.6 weight %. The upper limit is preferably 3 weight %, and particularly preferably 2 weight %).
[0079]
[34] The screen printing ink according to any one of
[18] to
[32] , wherein the content of the compound represented by the general formula (b') is 5 to 10 wt% (preferably 5 to 8.5 wt%) in the total amount of the screen printing ink (100 wt%).
[0080]
[35] The screen printing ink according to any one of [1] to
[34] , which has a viscosity of 10 to 100 Pa·s at 25°C and a shear rate of 100 (1 / s) (the upper limit is preferably 80 Pa·s, particularly preferably 60 Pa·s, most preferably 50 Pa·s, and extremely preferably 40 Pa·s. The lower limit is preferably 15 Pa·s, particularly preferably 20 Pa·s, most preferably 25 Pa·s, and extremely preferably 30 Pa·s).
[0081]
[36] The screen printing ink according to any one of [1] to
[35] , which has a TI value at 25°C (viscosity at a shear rate of 10 (1 / s) / viscosity at a shear rate of 100 (1 / s)) of 3.0 to 10.0 (preferably 3.5 to 7.0, particularly preferably 4.0 to 6.5, most preferably 4.5 to 6.3, and extremely preferably 4.8 to 6.2).
[0082]
[37] The screen printing ink according to any one of [1] to
[36] , wherein
[0083] The volume resistivity of the sintered body obtained by sintering at 120° C. for 30 minutes is 10 μΩcm or less (preferably 8 μΩcm or less, particularly preferably 6 μΩcm or less).
[0084]
[38] A method for manufacturing an electronic device, comprising: a step of applying the screen printing ink described in any one of [1] to
[37] onto a substrate by screen printing; and a step of sintering.
[0085]
[39] An electronic device having a sintered body of the screen printing ink according to any one of [1] to
[37] on a substrate thereof.
[0086] Effects of the Invention
[0087] Since the ink of the present invention has the technical features, when the ink is used, it is possible to draw high-precision fine lines by screen printing. In addition, since the volatility of the ink at the printing temperature is extremely low, the mesh clogging of the screen plate is suppressed, and continuous printing (for example, continuous printing more than 40 times) can be performed. In addition, the ink of the present invention is applied and then sintered (even if it is low-temperature sintering), thereby obtaining a sintered body with excellent conductivity. Therefore, the ink of the present invention is applicable to the use of manufacturing electronic components (for example, electrodes or wiring, etc.) on plastic substrates using screen printing. DETAILED DESCRIPTION
[0088] [Inks for screen printing]
[0089] The screen printing ink of the present invention comprises the following surface-modified silver nanoparticles (A) and the following solvent (B), and has a viscosity (at 25° C. and a shear rate of 10 (1 / s)) of 60 Pa·s or more.
[0090] Surface-modified silver nanoparticles (A): silver nanoparticles having a structure in which the surface is coated with an amine-containing protective agent.
[0091] Solvent (B): contains at least a terpene solvent, and the content of the solvent having a boiling point lower than 130° C. is 20% by weight or less of the total amount of the solvent.
[0092] (Surface modified silver nanoparticles (A))
[0093] The surface-modified silver nanoparticles of the present invention have a structure in which the surface of the silver nanoparticles is coated with an amine-containing protective agent, and more specifically, have a structure in which the unshared electron pairs of the amines are electrically coordinated on the surface of the silver nanoparticles. Since the screen printing ink of the present invention contains the surface-modified silver nanoparticles as a conductive material, it has excellent dispersion stability.
[0094] In the surface-modified silver nanoparticles of the present invention, the average primary particle size of the silver nanoparticle portion is, for example, 0.5 to 100 nm, preferably 0.5 to 80 nm, more preferably 1 to 70 nm, and even more preferably 1 to 60 nm.
[0095] (Solvent (B))
[0096] The solvent (B) in the present invention contains at least a terpene solvent, and the content of the solvent having a boiling point of less than 130° C. is 20% by weight or less of the total amount of the solvent. Since the screen printing ink of the present invention contains the solvent (B), clogging of the mesh of the screen plate caused by volatilization of the solvent is suppressed, thereby enabling continuous printing.
[0097] The terpene solvent is preferably a solvent having a boiling point of 130° C. or higher (eg, 130 to 300° C., preferably 200 to 300° C.).
[0098] In addition, as the terpene solvent, it is preferred to use a solvent having a viscosity (at 20° C.) of, for example, 50 to 250 mPa·s (particularly preferably 100 to 250 mPa·s, and most preferably 150 to 250 mPa·s), which can appropriately increase the viscosity of the resulting screen printing ink and preferably enable fine lines to be drawn with excellent accuracy. It should be noted that the viscosity of the solvent is a value measured at 20° C. and a shear rate of 20 (1 / s) using a rheometer (trade name "Physica MCR 301", manufactured by Anton Paar).
[0099] As the terpene solvent, for example, 4-(1'-acetoxy-1'-methyl ester)-cyclohexanol acetate, 1,2,5,6-tetrahydrobenzyl alcohol, 1,2,5,6-tetrahydrobenzyl acetate, cyclohexyl acetate, 2-methylcyclohexyl acetate, 4-tert-butyl cyclohexyl acetate, terpineol, dihydroterpineol, dihydroacetic acid pine ester, α-pineol, β-terpineol, γ-terpineol, L-α-terpineol, dihydropine oil base oxyethanol, pine oil base methyl ether, dihydropine oil base methyl ether, etc. can be cited. They can be used alone or in combination of two or more. In the present invention, for example, the following commercial products can be used: trade name "Terusolve MTPH", "Terusolve IPG", "Terusolve IPG-Ac", "Terusolve IPG-2Ac", "Terpineol C" (a mixture of α-terpineol, β-terpineol, and γ-terpineol). "Terusolve DTO-210", "Terusolve THA-90", "Terusolve THA-70" (boiling point: 223°C, viscosity: 198 mPa·s), "Terusolve TOE-100" (all manufactured by Terpene Chemical Co., Ltd. of Japan), and the like.
[0100] The solvent (B) of the present invention may contain one or more other solvents in addition to the terpene solvents. Examples of the other solvents include glycol ether solvents having a boiling point of 130° C. or higher.
[0101] The glycol ether solvent includes, for example, a compound represented by the following general formula (b):
[0102] R 11 -(OR 13 ) m -OR 12 (b)
[0103] (In the general formula, R 11 and R 12 are the same or different and represent an alkyl group or an acyl group, R 13represents an alkylene group having 1 to 6 carbon atoms, and m represents an integer greater than 1).
[0104] As the R 11 and R 12 The alkyl group includes a linear or branched alkyl group having 1 to 10 (preferably 1 to 5) carbon atoms.
[0105] As R 11 and R 12 The acyl group (RCO-group) includes a straight chain or branched chain alkyl group having 1 to 10 (preferably 1 to 5) carbon atoms (for example, acetyl, propionyl, butyryl, isobutyryl, pivaloyl, etc.).
[0106] In the present invention, the following compounds are preferred: R 11 and R 12 are different groups (different alkyl groups, different acyl groups, or different alkyl groups and acyl groups), and the following compounds are particularly preferred: 11 and R 12 are different alkyl groups, and the most preferred compounds are: 11 and R 12 It is a combination of a linear or branched alkyl group having 4 to 10 (preferably 4 to 6) carbon atoms and a linear or branched alkyl group having 1 to 3 carbon atoms.
[0107] As the R 13 The alkylene group includes, for example, methylene, methylmethylene, dimethylmethylene, ethylene, propylene, trimethylene, tetramethylene, pentamethylene, hexamethylene, etc. In the present invention, an alkylene group having 1 to 4 carbon atoms is particularly preferred, an alkylene group having 1 to 3 carbon atoms is particularly preferred, and an alkylene group having 2 to 3 carbon atoms is most preferred.
[0108] m is an integer of 1 or more, for example, an integer of 1-8, preferably an integer of 1-3, and particularly preferably an integer of 2-3.
[0109] The compound represented by the general formula (b) has a boiling point of, for example, 130° C. or higher (eg, 130 to 300° C.), preferably 170° C. or higher, particularly preferably 200° C. or higher.
[0110] Examples of the compound represented by the general formula (b) include ethylene glycol methyl ether acetate (boiling point: 145° C.), ethylene glycol n-butyl ether acetate (boiling point: 188° C.), propylene glycol methyl n-propyl ether (boiling point: 131° C.), propylene glycol methyl n-butyl ether (boiling point: 155° C.), propylene glycol methyl isoamyl ether (boiling point: 176° C.), propylene glycol diacetate (boiling point: 190° C.), propylene glycol methyl ether acetate (boiling point: 146° C.), 3-methoxybutyl ether ester (boiling point: 171°C), 1,3-butanediol diacetate (boiling point: 232°C), 1,4-butanediol diacetate (boiling point: 232°C), 1,6-hexanediol diacetate (boiling point: 260°C), diethylene glycol dimethyl ether (boiling point: 162°C), diethylene glycol diethyl ether (boiling point: 189°C), diethylene glycol dibutyl ether (boiling point: 256°C), diethylene glycol ethyl methyl ether (boiling point: 176°C), diethylene glycol isopropyl methyl ether (boiling point: 189°C), diethylene glycol di ... diethyl ether (boiling point: 189°C), diethylene glycol dibutyl ether (boiling point: 256°C), diethylene glycol diethyl ether (boiling point: 189°C), diethylene glycol dibutyl ether (boiling point: 256°C), diethylene glycol diethyl ether (boiling point: 189°C), diethylene glycol dibutyl ether (boiling point: 256°C), diethylene glycol diethyl methyl ether (boiling point: 189°C), diethylene glycol dibutyl ether (boiling point: 256°C), diethylene glycol diethyl methyl ether (boiling point: 189°C), diethylene glycol dibutyl ether (boiling point: 189°C), diethylene glycol dibutyl ether ( Point: 179°C), diethylene glycol methyl n-butyl ether (boiling point: 212°C), diethylene glycol n-butyl ether acetate (boiling point: 247°C), diethylene glycol ethyl ether acetate (boiling point: 218°C), diethylene glycol butyl ether acetate (boiling point: 246.8°C), dipropylene glycol methyl isopentyl ether (boiling point: 227°C), dipropylene glycol dimethyl ether (boiling point: 175°C), dipropylene glycol methyl n-propyl ether (boiling point: 203°C), dipropylene glycol methyl n-butyl ether (boiling point: Glycol diethers, glycol ether acetates and glycol diacetates such as triethylene glycol dimethyl ether (boiling point: 216°C), dipropylene glycol methyl cyclopentyl ether (boiling point: 286°C), dipropylene glycol methyl ether acetate (boiling point: 195°C), triethylene glycol dimethyl ether (boiling point: 216°C), triethylene glycol methyl n-butyl ether (boiling point: 261°C), tripropylene glycol methyl n-propyl ether (boiling point: 258°C), tripropylene glycol dimethyl ether (boiling point: 215°C), and tetraethylene glycol dimethyl ether (boiling point: 275°C) can be used alone or in combination of two or more.
[0111] In addition, the glycol ether solvent may also include, for example, a compound represented by the following general formula (b'):
[0112] R 14 -(OR 15 ) n -OH (b')
[0113] (Where R 14 represents an alkyl or aryl group, R 15 represents an alkylene group having 1 to 6 carbon atoms, and n represents an integer greater than 1).
[0114] As R 14Examples of the alkyl group include linear or branched alkyl groups having 1 to 10 carbon atoms (preferably 1 to 5). Examples of the aryl group include aryl groups having 6 to 10 carbon atoms (for example, phenyl, etc.).
[0115] As the R 15 The alkylene group includes, for example, straight-chain or branched alkylene groups such as methylene, methylmethylene, dimethylmethylene, ethylene, propylene, trimethylene, tetramethylene, pentamethylene, and hexamethylene. In the present invention, an alkylene group having 1 to 4 carbon atoms is preferred, an alkylene group having 1 to 3 carbon atoms is particularly preferred, and an alkylene group having 2 to 3 carbon atoms is most preferred.
[0116] n is an integer of 1 or more, for example, an integer of 1 to 8, preferably an integer of 1 to 3, and particularly preferably an integer of 2 to 3.
[0117] The compound represented by the general formula (b') has a boiling point of, for example, 130°C or higher (eg, 130 to 310°C), preferably 130 to 250°C, particularly preferably 130 to 200°C, most preferably 130 to 180°C, and extremely preferably 140 to 180°C.
[0118] Examples of the compound represented by the general formula (b') include ethylene glycol monomethyl ether (boiling point: 124°C), ethylene glycol monoisopropyl ether (boiling point: 141.8°C), ethylene glycol monobutyl ether (boiling point: 171.2°C), ethylene glycol monoisobutyl ether (boiling point: 160.5°C), ethylene glycol mono-tert-butyl ether (boiling point: 152°C), ethylene glycol monohexyl ether (boiling point: 208°C), ethylene glycol mono-2-ethylhexyl ether (boiling point: 229°C), ethylene glycol monophenyl ether (boiling point: 244.7°C), ethylene glycol monobenzyl ether (boiling point: 256°C), diethylene glycol monomethyl ether (boiling point: 194°C), diethylene glycol monobutyl ether (=butyl carbitol, boiling point: 230°C), diethylene glycol monoisobutyl ether (boiling point: 220°C), diethylene glycol monotert-butyl ether (boiling point: 152°C), ethylene glycol monohexyl ether (boiling point: 208°C), ethylene glycol mono-2-ethylhexyl ether (boiling point: 229°C), ethylene glycol monophenyl ether (boiling point: 244.7°C), ethylene glycol monobenzyl ether (boiling point: 256°C), diethylene glycol monomethyl ether (boiling point: 194°C), diethylene glycol monobutyl ether (=butyl carbitol, boiling point: 230°C), diethylene glycol monoisobutyl ether (boiling point: 220°C), diethylene glycol monoisopropyl ether (boiling point: 207°C), diethylene glycol monopentyl ether (boiling point: 162°C), diethylene glycol monoisopentyl ether, diethylene glycol monohexyl ether (= hexyl carbitol, boiling point: 259.1°C), diethylene glycol mono-2-ethylhexyl ether (boiling point: 272°C), diethylene glycol monophenyl ether (boiling point: 283°C), diethylene glycol monobenzyl ether (boiling point: 302°C), triethylene glycol monomethyl ether (boiling point: 249°C), triethylene glycol monobutyl ether (boiling point: 271.2°C), propylene glycol monoethyl ether (boiling point: 132.8°C), propylene glycol monopropyl ether (boiling point: 149°C), propylene glycol monobutyl ether (boiling point: 170°C), dipropylene glycol monomethyl ether (boiling point: 188°C), 3-methoxy-1-butanol (boiling point: 158°C), etc. These may be used alone or in combination of two or more.
[0119] The screen printing ink of the present invention may contain, as a solvent having a boiling point of 130°C or higher, one or more other solvents [for example, ethyl lactate acetate (boiling point: 181°C), tetrahydrofurfuryl acetate (boiling point: 195°C), tetrahydrofurfuryl alcohol (boiling point: 176°C), ethylene glycol (boiling point: 197°C), etc.] in addition to the compound represented by the general formula (b) and the compound represented by the general formula (b'), but the content of the other solvent having a boiling point of 130°C or higher is 30% by weight or less, preferably 20% by weight or less, particularly preferably 15% by weight or less, most preferably 10% by weight, further preferably 5% by weight or less, and extremely preferably 1% by weight or less, based on the total amount of the solvent contained in the screen printing ink of the present invention.
[0120] (Other ingredients)
[0121] The screen printing ink of the present invention may contain additives such as a binder resin, a surface energy regulator, a plasticizer, a leveling agent, a defoamer, an adhesiveness imparting agent, etc., in addition to the above-mentioned components, as required. In the present invention, it is preferred to contain a binder resin (C) from the viewpoint of improving the adhesion and flexibility of a sintered body obtained by applying (or printing) the screen printing ink of the present invention on a substrate and then sintering it.
[0122] As the binder resin (C), for example, vinyl chloride-vinyl acetate copolymer resin, polyvinyl butyral resin, polyester resin, acrylic resin, cellulose resin, etc. can be cited. They can be used alone or in combination of two or more. In the present invention, it is preferred to use a cellulose resin, for example, commercial products such as trade names "Ethocel std.200", "Ethocel std.300" (above, manufactured by Dow Chemical Co., Ltd.) can be used.
[0123] The content of the binder resin (C) (for example, a cellulose resin) is, for example, about 0.5 to 5.0% by weight, preferably 1.0 to 3.0% by weight, based on the total amount of the screen printing ink.
[0124] (Method for producing screen printing ink)
[0125] The screen printing ink of the present invention can be prepared, for example, by the following steps: a step of mixing a silver compound and an amine-containing protective agent to generate a complex containing the silver compound and an amine (complex generation step); a step of thermally decomposing the complex (thermal decomposition step); and a step of washing the reaction product as needed (washing step) to produce surface-modified silver nanoparticles, and a step of mixing the obtained surface-modified silver nanoparticles (A) with a solvent (B) containing at least a terpene solvent (ink preparation step).
[0126] (Complex Formation Step)
[0127] As the silver compound, it is preferred to use a compound that is easily decomposed by heating to generate metallic silver. Examples of such silver compounds include silver carboxylates such as silver formate, silver acetate, silver oxalate, silver malonate, silver benzoate, and silver phthalate; silver halides such as silver fluoride, silver chloride, silver bromide, and iodide; silver sulfate, silver nitrate, and silver carbonate. In the present invention, silver oxalate is preferred because it has a high silver content, can be thermally decomposed without a reducing agent, easily generates metallic silver by decomposition, and impurities derived from the ink reducing agent are not easily mixed.
[0128] The amine is a compound obtained by replacing at least one hydrogen atom of ammonia with a hydrocarbon group, and includes primary amines, secondary amines, and tertiary amines. In addition, the amine may be a monoamine or a polyamine such as a diamine. They may be used alone or in combination of two or more.
[0129] As the amine, it is preferred to contain at least one selected from the following amines: a monoamine (1) having a total carbon number of 6 or more, which is represented by the following general formula (a-1), wherein R 1 , R 2 , R 3 are the same or different and are hydrogen atoms or monovalent hydrocarbon groups (except R 1 , R 2 , R 3 The total number of carbon atoms is 5 or less, and the monoamine (2) is represented by the following general formula (a-1), and R in the general formula is 1 , R 2 , R 3 are the same or different and are hydrogen atoms or monovalent hydrocarbon groups (except R 1 , R 2 , R 3 and a diamine (3) having a total carbon number of 8 or less, which is represented by the following general formula (a-2), and R in the general formula is 8 is a divalent hydrocarbon group, R 4 ~R 7 The amines are the same or different and each is a hydrogen atom or a monovalent hydrocarbon group. The amines particularly preferably contain the monoamine (1) and contain a monoamine (2) and / or a diamine (3).
[0130] [Chemical formula 2]
[0131]
[0132] The hydrocarbon group includes an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group, among which an aliphatic hydrocarbon group or an alicyclic hydrocarbon group is preferred, and an aliphatic hydrocarbon group is particularly preferred. Therefore, the monoamine (1), monoamine (2), and diamine (3) are preferably an aliphatic monoamine (1), an aliphatic monoamine (2), and an aliphatic diamine (3).
[0133] In addition, the monovalent aliphatic hydrocarbon group includes an alkyl group and an alkenyl group. The monovalent alicyclic hydrocarbon group includes a cycloalkyl group and a cycloalkenyl group. In addition, the divalent aliphatic hydrocarbon group includes an alkylene group and an alkenylene group, and the divalent alicyclic hydrocarbon group includes a cycloalkylene group and a cycloalkenylene group.
[0134] As R 1 , R 2 , R 3 The monovalent hydrocarbon group in the group includes, for example, alkyl groups having about 1 to 20 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, decyl, dodecyl, tetradecyl and octadecyl; alkenyl groups having about 2 to 20 carbon atoms, such as vinyl, allyl, methallyl, 1-propenyl, isopropenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl and 5-hexenyl; cycloalkyl groups having about 3 to 20 carbon atoms, such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl and cyclooctyl; cycloalkenyl groups having about 3 to 20 carbon atoms, such as cyclopentenyl and cyclohexenyl, and the like.
[0135] As R 4 ~R 7 The monovalent hydrocarbon group in the above-mentioned examples includes hydrocarbon groups having 7 or less carbon atoms.
[0136] As R 8 The divalent hydrocarbon group in the alkylene group includes, for example, alkylene groups having 1 to 8 carbon atoms such as methylene, methylmethylene, dimethylmethylene, ethylene, propylene, trimethylene, tetramethylene, pentamethylene and heptamethylene; and alkenylene groups having 2 to 8 carbon atoms such as vinylene, propenylene, 1-butenylene, 2-butenylene, butadienyl, pentenylene, hexenylene, heptenylene and octenylene.
[0137] The R 1 ~R 8 The hydrocarbon group may contain: various substituents [e.g., halogen atoms, oxo groups, hydroxyl groups, substituted oxy groups (e.g., C 1-4 Alkoxy, C 6-10 Aryloxy, C 7-16 Aralkyloxy, C 1-4 acyloxy, etc.), carboxyl, substituted oxycarbonyl (e.g., C 1-4 Alkoxycarbonyl, C 6-10 Aryloxycarbonyl, C7-16 The hydroxyl group or carboxyl group may be protected by a protecting group commonly used in the field of organic synthesis.
[0138] The monoamine (1) is a compound having the function of imparting high dispersibility to the silver nanoparticles, and examples thereof include: primary amines having a straight-chain alkyl group such as hexylamine, heptylamine, octylamine, nonylamine, decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, heptadecanamine, octadecylamine, etc.; primary amines having a branched alkyl group such as isohexylamine, 2-ethylhexylamine, tert-octylamine; primary amines having a cycloalkyl group such as cyclohexylamine; primary amines having an alkenyl group such as oleylamine, etc.; N,N-dipropylamine, N,N-dibutylamine, N,N- -Secondary amines having a straight-chain alkyl group, such as dipentylamine, N,N-dihexylamine, N,N-diheptylamine, N,N-dioctylamine, N,N-didecylamine, N,N-dinonylamine, N,N-diundecylamine, N,N-didodecylamine, and N-propyl-N-butylamine; secondary amines having a branched-chain alkyl group, such as N,N-diisohexylamine and N,N-di(2-ethylhexyl)amine; tertiary amines having a straight-chain alkyl group, such as tributylamine and trihexylamine; tertiary amines having a branched-chain alkyl group, such as triisohexylamine and tri(2-ethylhexyl)amine, etc.
[0139] Among the monoamines (1), in order to ensure a distance between the amino group and other silver nanoparticles when the amino group is adsorbed on the surface of the silver nanoparticles and to enhance the effect of preventing the silver nanoparticles from agglomerating with each other, preferably, an amine (particularly a primary amine) having a total carbon number of 6 or more (from the viewpoint of easy acquisition and easy removal during sintering, the upper limit of the total carbon number is preferably about 18, more preferably 16, and particularly preferably 12) and having a straight-chain alkyl group, and hexylamine, heptylamine, octylamine, nonylamine, decylamine, undecylamine, dodecylamine and the like are particularly preferred.
[0140] Furthermore, when an amine having a branched alkyl group (particularly a primary amine) is used among the monoamines (1), compared with the case of using an amine having a straight-chain alkyl group having the same total number of carbon atoms, a smaller amount of the silver nanoparticles can be provided with higher dispersibility due to the steric factor of the branched alkyl group. Therefore, the amine can be effectively removed during sintering, particularly at low temperature, so that a sintered body with better conductivity can be obtained, which is preferred.
[0141] As the amine having the branched alkyl group, amines having a branched alkyl group having a total carbon number of 6 to 16 (preferably 6 to 10) such as isohexylamine and 2-ethylhexylamine are particularly preferred. In particular, from the viewpoint of spatial factors, amines having a branched alkyl group such as 2-ethylhexylamine are effective, and the branched alkyl group has a structure branched at the second carbon atom from the nitrogen atom.
[0142] Since the hydrocarbon chain of monoamine (2) is shorter than that of monoamine (1), it is believed that the function of imparting high dispersibility to silver nanoparticles is relatively low. However, since the polarity of monoamine (2) is higher than that of monoamine (1), the coordination ability to silver atoms is higher, so monoamine (2) is believed to have a complex formation promoting effect. In addition, since the hydrocarbon chain is relatively short, it can be removed from the surface of silver nanoparticles in a short time (for example, 30 minutes or less, preferably 20 minutes or less) even during low-temperature sintering, and a sintered body with excellent conductivity can be obtained.
[0143] Examples of the monoamine (2) include primary amines having a linear or branched alkyl group with a total carbon number of 2 to 5, such as ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, sec-butylamine, tert-butylamine, pentylamine, isopentylamine, tert-pentylamine, etc.; and secondary amines having a linear or branched alkyl group with a total carbon number of 2 to 5, such as N,N-dimethylamine, N,N-diethylamine, N-methyl-N-propylamine, N-ethyl-N-propylamine, etc.
[0144] As monoamine (2), preferred are primary amines having a straight chain or branched alkyl group with a total carbon number of 2 to 5 (preferably a total carbon number of 4 to 5), such as n-butylamine, isobutylamine, sec-butylamine, tert-butylamine, pentylamine, isopentylamine, tert-pentylamine, and particularly preferred are primary amines having a straight chain or branched alkyl group with a total carbon number of 2 to 5 (preferably a total carbon number of 4 to 5).
[0145] The diamine (3) has a total carbon number of 8 or less (e.g., 1 to 8) and has a higher polarity than the monoamine (1), thereby having a higher coordination ability to silver atoms, and is therefore considered to have a complex formation promoting effect. In addition, the diamine (3) has an effect of promoting thermal decomposition at a lower temperature and in a shorter time in the thermal decomposition process of the complex, and the use of the diamine (3) enables more efficient production of silver nanoparticles. In addition, the surface-modified silver nanoparticles coated with a protective agent containing the diamine (3) exhibit excellent dispersion stability in a dispersion medium containing a highly polar solvent. In addition, since the hydrocarbon chain of the diamine (3) is relatively short, it can be removed from the surface of the silver nanoparticles in a short time (e.g., 30 minutes or less, preferably 20 minutes or less) even under low-temperature sintering, thereby obtaining a sintered body with excellent conductivity.
[0146] Examples of the diamine (3) include ethylenediamine, 1,3-propylenediamine, 2,2-dimethyl-1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,5-diamino-2-methylpentane, and the like. 4 ~R 7 is a hydrogen atom, R 8is a straight-chain or branched alkylene diamine; N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N'-dimethyl-1,3-propylenediamine, N,N'-diethyl-1,3-propylenediamine, N,N'-dimethyl-1,4-butanediamine, N,N'-diethyl-1,4-butanediamine, N,N'-dimethyl-1,6-hexanediamine, etc. 4 , R 6 are the same or different and are straight chain or branched chain alkyl groups, R 5 , R 7 is a hydrogen atom, R 8 is a straight-chain or branched alkylene diamine; N,N-dimethylethylenediamine, N,N-diethylethylenediamine, N,N-dimethyl-1,3-propylenediamine, N,N-diethyl-1,3-propylenediamine, N,N-dimethyl-1,4-butanediamine, N,N-diethyl-1,4-butanediamine, N,N-dimethyl-1,6-hexanediamine, etc. 4 , R 5 are the same or different and are straight chain or branched chain alkyl groups, R 6 , R 7 is a hydrogen atom, R 8 It is a straight chain or branched chain alkylene diamine, etc.
[0147] Among them, it is preferred that R in the general formula (a-2) 4 , R 5 are the same or different and are straight chain or branched chain alkyl groups, R 6 , R 7 is a hydrogen atom, R 8 is a linear or branched alkylene diamine [particularly, R in the general formula (a-2) 4 , R 5 is a straight chain alkyl group, R 6 , R 7 is a hydrogen atom, R 8 is a straight chain alkylene diamine].
[0148] R in the general formula (a-2) 4 , R 5 are the same or different and are straight chain or branched chain alkyl groups, R 6 , R 7The diamine is a diamine having a hydrogen atom, that is, a diamine having a primary amino group and a tertiary amino group, wherein the primary amino group has a high coordination ability for the silver atom, and the tertiary amino group has a low coordination ability for the silver atom, thereby preventing the formed complex from being excessively complicated, thereby enabling thermal decomposition at a lower temperature and in a short time in the thermal decomposition process of the complex. Among them, from the viewpoint of being able to be removed from the surface of the silver nanoparticles in a short time under low-temperature sintering, a diamine having a total carbon number of 6 or less (e.g., 1 to 6) is preferred, and a diamine having a total carbon number of 5 or less (e.g., 1 to 5) is more preferred.
[0149] When the amine of the present invention contains a monoamine (1) and a monoamine (2) and / or a diamine (3) in combination, the ratio of these amines to be used is not particularly limited, but is preferably in the following range based on the total amount of amines [monoamine (1) + monoamine (2) + diamine (3); 100 mol %].
[0150] The content of the monoamine (1): for example, 5 to 65 mol% (the lower limit is preferably 10 mol%, particularly preferably 15 mol%). The upper limit is preferably 50 mol%, particularly preferably 40 mol%, and most preferably 35 mol%)
[0151] The total content of the monoamine (2) and the diamine (3): for example, 35 to 95 mol% (the lower limit is preferably 50 mol%, particularly preferably 60 mol%, and most preferably 65 mol%. The upper limit is preferably 90 mol%, particularly preferably 85 mol%)
[0152] When monoamine (2) and diamine (3) are used together, the content of each of monoamine (2) and diamine (3) is preferably within the following ranges based on the total amount of amines [monoamine (1) + monoamine (2) + diamine (3); 100 mol %].
[0153] Monoamine (2): for example, 5 to 70 mol% (the lower limit is preferably 10 mol%, particularly preferably 15 mol%. The upper limit is preferably 65 mol%, particularly preferably 60 mol%).
[0154] Diamine (3): for example, 5 to 50 mol% (the lower limit is preferably 10 mol%. The upper limit is preferably 45 mol%, particularly preferably 40 mol%).
[0155] By containing the monoamine (1) within the above range, the dispersion stability of the silver nanoparticles can be obtained. When the content of the monoamine (1) is less than the above range, there is a tendency that it is difficult to obtain the dispersion stability of the silver nanoparticles. On the other hand, when the content of the monoamine (1) is greater than the above range, there is a tendency that it is difficult to remove the amine by low-temperature sintering.
[0156] By containing the monoamine (2) within the above range, the complex formation promoting effect can be easily obtained. In addition, sintering can be performed at a low temperature and in a short time, and the diamine (3) can be easily removed from the surface of the silver nanoparticles during sintering.
[0157] By containing the monoamine (3) within the above range, the complex formation promoting effect and the complex thermal decomposition promoting effect are easily obtained. In addition, the surface-modified silver nanoparticles having a structure coated with a protective agent containing diamine (3) show excellent dispersion stability in a dispersion medium containing a highly polar solvent.
[0158] In the present invention, when monoamine (2) and / or diamine (3) having a high coordination ability for silver atoms of a silver compound is used, the amount of monoamine (1) used is reduced according to their usage ratio. Under the condition of low temperature and short sintering time, these amines are easily removed from the surface of silver nanoparticles, and the sintering of silver nanoparticles can be fully carried out.
[0159] The amines used as the protective agent in the present invention may contain other amines in addition to the monoamine (1), the monoamine (2) and the diamine (3), but the total content of the monoamine (1), the monoamine (2) and the diamine (3) in the total amines contained in the protective agent is preferably 60% by weight or more, particularly preferably 80% by weight or more, and most preferably at least 90% by weight. The upper limit is 100% by weight. That is, the content of other amines is preferably 60% by weight or less, particularly preferably 20% by weight or less, and most preferably 10% by weight or less.
[0160] The amount of the amines [especially, monoamine (1) + monoamine (2) + diamine (3)] used is not particularly limited, but is preferably about 1 to 50 mol per 1 mol of the silver atom of the silver compound as a raw material, preferably 2 to 50 mol, and particularly preferably 6 to 50 mol from the viewpoint of obtaining surface-modified silver nanoparticles in the substantial absence of a solvent. When the amount of the amines used is less than the above range, the silver compound that has not been converted into a complex is likely to remain in the complex formation step, and in the subsequent thermal decomposition step, the uniformity of the silver nanoparticles is impaired, causing the particles to become enlarged. Since the silver compound may remain without being thermally decomposed, this is not preferred.
[0161] The reaction of the amine and the silver compound is carried out in the presence or absence of a solvent. As the solvent, for example, an alcohol solvent having 3 or more carbon atoms can be used.
[0162] Examples of the alcohol solvent include n-propanol (boiling point: 97° C.), isopropanol (boiling point: 82° C.), n-butanol (boiling point: 117° C.), isobutanol (boiling point: 107.89° C.), sec-butanol (boiling point: 99.5° C.), tert-butanol (boiling point: 82.45° C.), n-pentanol (boiling point: 136° C.), n-hexanol (boiling point: 156° C.), n-octanol (boiling point: 194° C.), and 2-octanol (boiling point: 174° C.). Among them, alcohol solvents having 4 to 6 carbon atoms are preferred, and n-butanol and n-hexanol are particularly preferred, from the viewpoint of being able to set a higher thermal decomposition step of the complex to be performed later and the convenience in the post-treatment of the obtained surface-modified silver nanoparticles.
[0163] In addition, the amount of the solvent used relative to 100 parts by weight of the silver compound is, for example, 120 parts by weight or more, preferably 130 parts by weight or more, and more preferably 150 parts by weight or more. It should be noted that the upper limit of the amount of the solvent used is, for example, 1000 parts by weight, preferably 800 parts by weight, and particularly preferably 500 parts by weight.
[0164] In the present invention, in order to further improve the dispersibility of the silver nanoparticles, one or more aliphatic monocarboxylic acids may be further used as protective agents. The use of aliphatic monocarboxylic acids tends to improve the stability of the silver nanoparticles, especially the stability in the state of being dispersed in the solvent (B).
[0165] Examples of the aliphatic monocarboxylic acid include saturated aliphatic monocarboxylic acids having 4 or more carbon atoms, such as butyric acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid, tetradecanoic acid, pentadecanoic acid, hexadecanoic acid, heptadecanoic acid, octadecanoic acid, nonadecanoic acid, and eicosanoic acid; and unsaturated aliphatic monocarboxylic acids having 8 or more carbon atoms, such as oleic acid, elaidic acid, linoleic acid, palmitoleic acid, and eicosenoic acid.
[0166] Among them, saturated or unsaturated aliphatic monocarboxylic acids with 8 to 18 carbon atoms (especially octanoic acid, oleic acid, etc.) are preferred. When the carboxyl group of the carboxylic aliphatic monocarboxylic acid is adsorbed on the surface of the silver nanoparticles, the saturated or unsaturated aliphatic hydrocarbon chain with 8 to 18 carbon atoms causes steric hindrance, thereby ensuring the spacing between other silver nanoparticles and improving the effect of preventing the silver nanoparticles from agglomerating with each other. In addition, the aliphatic monocarboxylic acid is easy to obtain and easy to remove during sintering, which is preferred in this regard.
[0167] The amount of the aliphatic monocarboxylic acid used is, for example, about 0.05 to 10 mol, preferably 0.1 to 5 mol, and particularly preferably 0.5 to 2 mol, relative to 1 mol of silver atoms in the silver compound. When the amount of the aliphatic monocarboxylic acid used is less than the above range, it is difficult to obtain the effect of improving stability. On the other hand, even if the aliphatic monocarboxylic acid is used in excess, the effect of improving the dispersion stability has reached saturation, and there is a tendency to be difficult to remove by low-temperature sintering.
[0168] The reaction between the amine-containing protective agent and the silver compound is preferably carried out at room temperature (5 to 40° C.). Since the reaction is accompanied by heat generated by the coordination reaction of the amine to the silver compound, the reaction can be carried out while appropriately cooling so as to be within the temperature range.
[0169] The reaction time between the amine-containing protective agent and the silver compound is, for example, about 30 minutes to 3 hours. Thus, a silver-amine complex is obtained.
[0170] (Thermal Decomposition Process)
[0171] The thermal decomposition step is a step of thermally decomposing the silver-amine complex obtained in the complex formation step to form surface-modified silver nanoparticles. By heating the silver-amine complex, the silver compound is thermally decomposed to generate silver atoms while maintaining the coordination bond of the amine to the silver compound, and then the silver atoms coordinated with the amine are condensed to form silver nanoparticles covered by an amine protective film (which plays a role in preventing the silver nanoparticles from re-aggregating with each other).
[0172] The thermal decomposition is preferably carried out in the presence of a solvent, and as a solvent, the alcohol solvent can be appropriately used. In addition, the thermal decomposition temperature can be any temperature at which surface-modified silver nanoparticles are generated. When the silver-amine complex is a silver oxalate-amine complex, it is, for example, about 80 to 120° C., preferably 95 to 115° C., and particularly preferably 100 to 110° C. From the viewpoint of preventing the surface-modified part of the surface-modified silver nanoparticles from detaching, it is preferably carried out at a temperature as low as possible within the temperature range. The thermal decomposition time is, for example, about 10 minutes to 5 hours.
[0173] Furthermore, the thermal decomposition of the silver-amine complex is preferably performed in an air atmosphere or an inert gas atmosphere such as argon.
[0174] (Cleaning process)
[0175] After the thermal decomposition reaction of the silver-amine complex is completed, when there is an excess protective agent (e.g., amine), it is preferred to perform decantation once, or to repeat the decantation twice or more, in order to remove the excess protective agent. In addition, after the decantation is completed, the surface-modified silver nanoparticles are used in the ink preparation process described later in a wet state without drying or curing, so that the re-agglomeration of the silver nanoparticles can be suppressed, which is preferred from the viewpoint of maintaining the high dispersibility of the silver nanoparticles.
[0176] In the case where the surface-modified silver nanoparticles are not dried and solidified, the cleaning solvent used in the decantation is inevitably mixed into the screen printing ink of the present invention. Therefore, as a cleaning solvent, when it is repeated twice or more, especially as the last cleaning solvent, it is preferred to use a solvent that does not damage the properties of the screen printing ink of the present invention. From the viewpoint of excellent cleaning properties and not damaging the high dispersibility of the silver nanoparticles and the continuous printing properties of the ink, it is preferred to use the compound represented by the general formula (b'). In addition, among the compounds represented by the general formula (b'), when a compound having a boiling point of, for example, 130 to 200°C, preferably 130 to 180°C, and particularly preferably 140 to 180°C is used, it is preferred that the cleaning properties are excellent and the high dispersibility of the silver nanoparticles and the continuous printing properties of the ink are not damaged, and the conductivity of the resulting sintered body is particularly excellent.
[0177] The decantation is performed by, for example, a method in which the surface-modified silver nanoparticles in a suspended state are washed with a washing solvent, precipitated by centrifugal separation, and the supernatant is removed.
[0178] The proportion of the cleaning solvent in the total amount of the wet surface-modified silver nanoparticles obtained by decantation is, for example, about 5 to 15 wt %. Therefore, the proportion of the surface-modified silver nanoparticles in the total amount of the wet surface-modified silver nanoparticles is, for example, about 85 to 95 wt %.
[0179] (Ink preparation process)
[0180] The ink preparation process is a process of mixing the surface-modified silver nanoparticles (A) obtained by the above process (preferably the surface-modified silver nanoparticles (A) wetted by the washing solvent), a solvent (B) containing at least a terpene solvent, and necessary additives to obtain the screen printing ink of the present invention. In the mixing, for example, conventionally known mixing equipment such as a self-rotating stirring defoaming device, a homogenizer, a planetary mixer, a three-roll mill, a bead mill, etc. can be used. In addition, the components can be mixed simultaneously or sequentially.
[0181] The mixing ratio of each component can be appropriately adjusted within the following range in which the screen printing ink can be obtained.
[0182] In the total amount (100 wt %) of the screen printing ink of the present invention, the content of the surface-modified silver nanoparticles is, for example, 60 to 85 wt %, and from the viewpoint of obtaining an effect of improving adhesion to the substrate, the lower limit is preferably 70 wt %. The upper limit is preferably 80 wt %, and particularly preferably 75 wt %.
[0183] In the total amount (100 wt%) of the screen printing ink of the present invention, the content of the terpene solvent is, for example, 5 to 30 wt%, with a lower limit of preferably 10%, particularly preferably 14 wt%. The upper limit is preferably 25 wt%, particularly preferably 18 wt%. By containing the terpene solvent within the above range, it is possible to suppress smearing, obtain an effect of improving the drawing accuracy of fine lines, and an effect of improving continuous printing properties.
[0184] In the total amount (100 wt%) of the screen printing ink of the present invention, the content of the compound represented by the general formula (b) is, for example, 0.5 to 5 wt%, and the lower limit is preferably 1.6 wt%. The upper limit is preferably 3 wt%, and particularly preferably 2 wt%. By containing the compound represented by the general formula (b) within the above range, thixotropy can be imparted, the edge of the drawing portion can be made clearer, and the printing accuracy can also be improved. In addition, the effect of improving continuous printing can be obtained.
[0185] The screen printing ink of the present invention may contain the compound represented by the general formula (b') in an amount of, for example, 10 wt % or less (5 to 10 wt %), preferably 8.5 wt % or less, based on the total amount of the ink.
[0186] In addition, the screen printing ink of the present invention may contain a solvent having a boiling point of less than 130°C [for example, ethylene glycol dimethyl ether (boiling point: 85°C), propylene glycol monomethyl ether (boiling point: 120°C), propylene glycol dimethyl ether (boiling point: 97°C), etc.], but the content of the solvent having a boiling point of less than 130°C (the total amount when two or more kinds are contained) in the total amount (100% by weight) of the screen printing ink of the present invention is 20% by weight, preferably 10% by weight or less, particularly preferably 5% by weight or less, and most preferably 1% by weight or less. As for the screen printing ink of the present invention, since the content of the solvent having a boiling point of less than 130°C is suppressed within the above range, the clogging of the screen plate caused by the volatilization of the solvent can be suppressed, and continuous printing can be performed.
[0187] The viscosity of the screen printing ink of the present invention (at 25° C. and a shear rate of 10 (1 / s)) is 60 Pa·s or more, preferably 70 Pa·s or more, more preferably 80 Pa·s or more, further preferably 90 Pa·s or more, further preferably 100 Pa·s or more, and particularly preferably 150 Pa·s or more. The upper limit of the viscosity is, for example, about 500 Pa·s, preferably 450 Pa·s, particularly preferably 400 Pa·s, and most preferably 350 Pa·s.
[0188] The viscosity of the screen printing ink of the present invention (at 25° C. and a shear rate of 10 (1 / s)) is, for example, 10 to 100 Pa·s, with an upper limit of preferably 80 Pa·s, particularly preferably 60 Pa·s, most preferably 50 Pa·s, and extremely preferably 40 Pa·s. The lower limit is preferably 15 Pa·s, particularly preferably 20 Pa·s, most preferably 25 Pa·s, and extremely preferably 30 Pa·s.
[0189] The screen printing ink of the present invention preferably has thixotropy, and the TI value (viscosity at a shear rate of 10 (1 / s) / viscosity at a shear rate of 100 (1 / s)) at 25°C is, for example, 3.0 to 10.0, preferably 3.5 to 7.0, particularly preferably 4.0 to 6.5, most preferably 4.5 to 6.3, and extremely preferably in the range of 4.8 to 6.2.
[0190] The screen printing ink of the present invention has excellent dispersion stability. For example, when the screen printing ink having a silver concentration of 65 wt % is stored at 5° C., an increase in viscosity can be suppressed for more than one month.
[0191] [Method for manufacturing electronic device]
[0192] The method for manufacturing an electronic device of the present invention comprises a step of applying the ink on a substrate by screen printing, and a step of sintering.
[0193] Since the screen printing ink is used in the method for manufacturing an electronic device of the present invention, sintering can be performed at a low temperature, and the sintering temperature is, for example, 130° C. or less (the sintering temperature is adjusted to, for example, 60° C., and from the viewpoint of being able to sinter in a short time, 100° C. is more preferred), and 120° C. or less is particularly preferred. The sintering time is, for example, 0.5 to 3 hours, preferably 0.5 to 2 hours, and particularly preferably 0.5 to 1 hour.
[0194] If the screen printing ink of the present invention is used, the sintering of the silver nanoparticles is fully carried out even at low temperature sintering (preferably low temperature and short time sintering). As a result, a sintered body having excellent conductivity, i.e., a volume resistivity of, for example, 10 μΩcm or less, preferably 8 μΩcm or less, and particularly preferably 6 μΩcm or less can be obtained. It should be noted that the conductivity (or volume resistivity) of the sintered body can be measured by the method described in the examples.
[0195] Since low-temperature sintering can be performed by using the screen printing ink of the present invention, in addition to heat-resistant plastic substrates such as glass substrates and polyimide films, general-purpose plastic substrates with low heat resistance such as polyester films such as polyethylene terephthalate (PET) films and polyethylene naphthalate (PEN) films, and polyolefin films such as polypropylene can also be appropriately used as substrates.
[0196] Electronic devices obtained by the method for manufacturing an electronic device of the present invention include, for example, liquid crystal displays, organic EL displays, field emission displays (FEDs), IC cards, IC tags, solar cells, LED elements, organic transistors, storage devices (capacitors), electronic paper, flexible batteries, flexible sensors, membrane switches, touch panels, EMI shielding, etc.
[0197] Example
[0198] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.
[0199] Preparation Example 1 (Preparation of surface-modified silver nanoparticles (1))
[0200] Silver oxalate (molecular weight: 303.78) was obtained from silver nitrate (manufactured by Wako Pure Chemical Industries, Ltd.) and oxalic acid dihydrate (manufactured by Wako Pure Chemical Industries, Ltd.).
[0201] 40.0 g (0.1317 mol) of the silver oxalate was added to a 500 mL flask, and 60 g of n-butanol was added thereto to prepare n-butanol slurry of silver oxalate. At 30° C., the following amine mixed solution was added dropwise to the slurry: n-butylamine (molecular weight: 73.14, reagent manufactured by Tokyo Chemical Industry Co., Ltd.) 115.58 g (1.5802 mol), 2-ethylhexylamine (molecular weight: 129.25, reagent manufactured by Wako Pure Chemical Industries, Ltd.) 51.06 g (0.3950 mol), and n-octylamine (molecular weight 129.25, reagent manufactured by Tokyo Chemical Industry Co., Ltd.) 17.02 g (0.1317 mol). After the addition, the mixture was stirred at 30° C. for 1 hour to perform a complex reaction between the silver oxalate and the amine. After the silver oxalate-amine complex was formed, the silver oxalate-amine complex was thermally decomposed by heating at 110° C. for 1 hour to obtain a suspension containing dark blue surface-modified silver nanoparticles.
[0202] The obtained suspension was cooled, and 120 g of methanol (a reagent manufactured by Wako Pure Chemical Industries, Ltd., special grade) was added thereto and stirred, and then the surface-modified silver nanoparticles were precipitated by centrifugation, and the supernatant was removed. 120 g of butyl carbitol (a reagent manufactured by Tokyo Chemical Industry Co., Ltd.) was then added to the surface-modified silver nanoparticles and stirred, and then the surface-modified silver nanoparticles were precipitated by centrifugation, and the supernatant was removed. Thus, wet surface-modified silver nanoparticles (1) containing butyl carbitol were obtained. From the results of a thermal balance using TG / DTA6300 manufactured by SII Corporation, the content of the surface-modified silver nanoparticles was 90% by weight in the total amount (100% by weight) of the wet surface-modified silver nanoparticles. That is, the wet surface-modified silver nanoparticles contained 10% by weight of butyl carbitol.
[0203] In addition, the surface-modified silver nanoparticles in a wet state were observed using a scanning electron microscope (JSM-6700F manufactured by JEOL Ltd.), and the particle sizes of 10 silver nanoparticles randomly selected in the SEM photograph were obtained, and the average value thereof was taken as the average particle size. The average particle size (primary particle size) of the silver nanoparticle portion in the surface-modified silver nanoparticles was about 50 nm.
[0204] Preparation Example 2 (Preparation of surface-modified silver nanoparticles (2))
[0205] Surface-modified silver nanoparticles (2) in a wet state containing 10 wt % of propylene glycol monobutyl ether were obtained in the same manner as in Preparation Example 1 except that propylene glycol monobutyl ether was used instead of butyl carbitol.
[0206] Preparation Example 3 (Preparation of surface-modified silver nanoparticles (3))
[0207] Surface-modified silver nanoparticles (3) in a wet state containing 10 wt % of propylene glycol monopropyl ether were obtained in the same manner as in Preparation Example 1 except that propylene glycol monopropyl ether was used instead of butyl carbitol.
[0208] Preparation Example 4 (Preparation of surface-modified silver nanoparticles (4))
[0209] Surface-modified silver nanoparticles (4) in a wet state containing 10 wt % of 3-methoxy-1-butanol were obtained in the same manner as in Preparation Example 1 except that 3-methoxy-1-butanol was used instead of butyl carbitol.
[0210] Preparation Example 5 (Preparation of surface-modified silver nanoparticles (5))
[0211] Surface-modified silver nanoparticles (5) in a wet state containing 10 wt % of propylene glycol monoethyl ether were obtained in the same manner as in Preparation Example 1 except that propylene glycol monoethyl ether was used instead of butyl carbitol.
[0212] Preparation Example 6 (Preparation of surface-modified silver nanoparticles (6))
[0213] Surface-modified silver nanoparticles (6) in a wet state containing 10 wt % of ethylene glycol mono-tert-butyl ether were obtained in the same manner as in Preparation Example 1 except that ethylene glycol mono-tert-butyl ether was used instead of butyl carbitol.
[0214] Example 1 (Preparation of Silver Ink)
[0215] THA-70, DPMIA, and EC300 were added, stirred in an oil bath (100 rpm) for 3 hours, and then stirred and kneaded in a rotary kneader (Mazerustar KKK2508, manufactured by Kurabo Co., Ltd.) (2 minutes x 3 times) to prepare Liquid A.
[0216] The wet surface-modified silver nanoparticles (1) obtained in Preparation Example 1 (containing 10 wt % of butyl carbitol) were added to Liquid A, and stirred and kneaded (2 minutes x 3 times) in a rotary kneader (Mazerustar KKK2508, manufactured by Kurabo Co., Ltd.) to obtain a dark brown silver ink.
[0217] Examples 2 to 6, Comparative Examples 1 to 4
[0218] The same procedure as in Example 1 was carried out except that the formulation was changed as shown in the following Table 1 (unit: parts by weight).
[0219] The printability, continuous printability, fine line drawing property, and conductivity and substrate adhesion of the silver inks obtained in Examples 2 to 6 and Comparative Examples 1 to 4 were evaluated by the following methods.
[0220] (Printability Evaluation)
[0221] The printability of the silver inks obtained in Examples 2 to 6 and Comparative Examples 1 to 4 was evaluated according to the following criteria.
[0222] ○: High-precision printing is possible by screen printing
[0223] △: Printing is possible by screen printing, but there is smearing or line breakage
[0224] X: Cannot be printed by screen printing
[0225] (Continuous printing evaluation)
[0226] The silver inks obtained in Examples 2 to 6 and Comparative Examples 1 to 4 were printed on a PET film at 25° C. using a screen printing device (manufactured by New Long Precision Industry Co., Ltd., LS-150TV). The continuous printing property was evaluated as good (○) when the number of continuous printings was 40 or more, and the continuous printing property was evaluated as poor (X) when the number of continuous printings was less than 40.
[0227] (Thin line drawing performance evaluation)
[0228] The silver inks obtained in Examples 2 to 6 and Comparative Examples 1 to 4 were printed on a PET film at 25° C. using a screen printing machine (manufactured by New Long Precision Industry Co., Ltd., LS-150TV), and the fine line drawing property was evaluated based on the minimum value of the line width of a fine line that could be drawn with high precision.
[0229] (Evaluation of electrical conductivity of sintered body)
[0230] The silver inks obtained in Examples 2 to 6 and Comparative Examples 1 to 4 were applied on a soda glass plate to form a coating film. Immediately after the coating film was formed, the coating film was sintered in an air drying oven at 120° C. for 30 minutes to obtain a sintered body having a thickness of about 2 μm. The conductivity of the obtained sintered body was measured by using a four-terminal method (Loresta GP MCP-T610) to measure the volume resistivity and evaluate the conductivity of the sintered body.
[0231] (Evaluation of adhesion between sintered body and substrate)
[0232] The soda glass plate / sintered body obtained by the same method as the conductivity evaluation was used as a sample. The sample was subjected to a tape peeling test (based on JIS K 5600), and the adhesion of the sintered body to the substrate was evaluated by evaluating the case where 100% of the sintered body remained as good adhesion (○), the case where 60% or more and less than 100% remained as slightly poor adhesion (△), and the case where less than 60% remained as poor adhesion (X).
[0233]
[0234] THA-70: 4-(1'-acetoxy-1'-methyl)-cyclohexanol acetate, trade name "Terusolve THA-70", manufactured by Terpene Chemical Co., Ltd., Japan, boiling point: 223°C, viscosity: 198 mPa·s
[0235] Dihydroterpineol: manufactured by Terpene Chemical Co., Ltd., Japan, boiling point: 210°C, viscosity (20°C): 83 mPa·s
[0236] Dihydropinyl acetate: manufactured by Terpene Chemical Co., Ltd., Japan, boiling point: 220-225°C, viscosity (20°C): 7 mPa·s
[0237] DPMIA: dipropylene glycol-methyl-isoamyl ether, boiling point: 227° C., manufactured by Daicel Corporation.
[0238] p-Terpane: 1-methyl-4-(1-methylethyl)cyclohexane, manufactured by Terpene Chemical Co., Ltd., Japan, boiling point: 168°C.
[0239] TOE-100: 2-(1-methyl-1-(4-methyl-3-cyclohexenyl)ethoxy)ethanol, trade name "Terusolve TOE-100", manufactured by Terpene Chemical Co., Ltd., Japan, boiling point: 268 to 282°C.
[0240] EC300: ethyl cellulose resin, trade name "Ethocel std.300 (ETHOCEL TM , std.300)", manufactured by Dow Chemical Co., Ltd.
[0241] Embodiments 7 to 11
[0242] Silver ink was obtained by using the wet surface-modified silver nanoparticles (2) to (6) obtained in Preparation Examples 2 to 6 instead of the wet surface-modified silver nanoparticles (1) (containing 10 wt % of butyl carbitol) and performing the same operation as in Example 1 except changing the content of each component as described in the following Table 2 (unit: parts by weight).
[0243] The silver inks obtained in Examples 7 to 11 were applied on a soda glass plate to form a coating film. Immediately after the coating film was formed, the coating film was sintered using a hot plate at 120° C. for 30 minutes to obtain a sintered body, and the volume resistivity of the obtained sintered body was measured by the same method as above.
[0244] [Table 2]
[0245]
[0246] Embodiments 12 to 16
[0247] Except that the mixing ratio was changed as described in Table 3 (unit: parts by weight), the same manner as in Example 9 was carried out to obtain a silver ink.
[0248] The silver inks obtained in Examples 12 to 16 were applied on a soda glass plate to form a coating film. Immediately after the coating film was formed, the coating film was sintered using a hot plate at 120° C. for 30 minutes to obtain a sintered body, and the volume resistivity of the obtained sintered body was measured by the same method as above.
[0249] [Table 3]
[0250]
[0251] From Tables 2 and 3, it can be found that when a glycol ether solvent having a boiling point of 130 to 200° C. is used as the glycol ether solvent, the thixotropy is enhanced compared to the case of using a glycol ether solvent having a boiling point exceeding 200° C., and a sintered body having further excellent conductivity is obtained. In addition, it was found that by adjusting the amount of EC 300 added as the binder resin, it is possible to maintain high conductivity and control the viscosity within a desired range.
[0252] Industrial Applicability
[0253] By using the ink of the present invention, fine lines can be drawn with high precision by screen printing. In addition, since the volatility of the ink at the printing temperature is extremely low, the mesh clogging of the screen is suppressed, and continuous printing can be performed for more than 40 times. In addition, after applying the ink of the present invention, a sintered body with excellent conductivity can be obtained by sintering. Therefore, the ink of the present invention can be applied to the use of manufacturing electronic components on a plastic substrate by screen printing.
Claims
1. A screen printing ink comprising the following surface-modified silver nanoparticles (A) and the following solvent (B), wherein the viscosity of the screen printing ink at 25° C. and a shear rate of 10 1 / s is 60 Pa·s or more, Surface-modified silver nanoparticles (A): having a structure in which the surface of the silver nanoparticles is coated with an amine-containing protective agent. Solvent (B): contains a terpene solvent and a glycol ether solvent having a boiling point of 130°C or higher, and the content of the solvent having a boiling point lower than 130°C is 5% by weight or less of the total amount of solvent contained in the ink, The surface-modified silver nanoparticles (A) are surface-modified silver nanoparticles in a wet state obtained by decantation using a washing solvent, wherein the washing solvent contains a compound represented by the following formula (b'), and the surface-modified silver nanoparticles account for 85 to 95% by weight of the total amount of the surface-modified silver nanoparticles in the wet state. R 14 -(O-R 15 ) n -OH(b’) In formula (b'), R 14 represents an alkyl or aryl group, R 15 represents an alkylene group having 1 to 6 carbon atoms, and n represents an integer greater than 1, The terpene solvent is a solvent selected from 4-(1'-acetoxy-1'-methyl ester)-cyclohexanol acetate, 1,2,5,6-tetrahydrobenzyl alcohol, 1,2,5,6-tetrahydrobenzyl acetate, cyclohexyl acetate, 2-methylcyclohexyl acetate, 4-tert-butyl cyclohexyl acetate, terpineol, dihydroterpineol, dihydroterpineol acetate, α-terpineol, β-terpineol, γ-terpineol, L-α-terpineol, dihydroterpineol oxyethanol, terpineol methyl ether, and dihydroterpineol methyl ether.
2. The screen printing ink according to claim 1, wherein The protective agent contains, as amines, an aliphatic monoamine (1) having a total carbon number of 6 or more, and an aliphatic monoamine (2) having a total carbon number of 5 or less and / or an aliphatic diamine (3) having a total carbon number of 8 or less.
3. The screen printing ink according to claim 2, wherein: The aliphatic monoamine (1) having a total carbon number of 6 or more is a monoamine having a linear alkyl group and having a total carbon number of 6 to 18 and / or a monoamine having a branched alkyl group and having a total carbon number of 6 to 16.
4. The screen printing ink according to claim 2 or 3, wherein The aliphatic monoamine (2) having a total carbon number of 5 or less is a monoamine having a linear or branched alkyl group and having a total carbon number of 2 to 5.
5. The screen printing ink according to claim 2 or 3, wherein The aliphatic diamine (3) having a total carbon number of 8 or less is represented by the following general formula (a-2): [Chemical formula 1] In the formula, R 4 and R 5 are the same or different and are straight chain or branched chain alkyl groups, R 6 and R 7 is a hydrogen atom, R 8 It is a straight chain or branched chain alkylene group.
6. The screen printing ink according to any one of claims 1 to 3, wherein The terpene-based solvent has a boiling point of 130° C. or higher and a viscosity of 50 to 250 mPa·s at 20° C.
7. The screen printing ink according to any one of claims 1 to 3, wherein The glycol ether solvent includes a compound represented by the following formula (b): R 11 -(O-R 13 ) m -OR 12 (b) In the formula, R 11 and R 12 are the same or different and represent an alkyl group or an acyl group, R 13 represents an alkylene group having 1 to 6 carbon atoms, and m represents an integer of 1 or greater. 8 . The screen printing ink according to claim 1 , further comprising a binder resin (C).
9. The screen printing ink according to any one of claims 1 to 3, wherein The volume resistivity of the sintered body obtained by sintering at 120° C. for 30 minutes was 10 μΩcm or less.
10. A method for manufacturing an electronic device, comprising: A step of applying the screen printing ink according to any one of claims 1 to 9 onto a substrate by screen printing; as well as, Sintering process. 11 . An electronic device comprising a sintered body of the screen printing ink according to claim 1 on a substrate.