Electromagnetic shielding protective film
The combination of a conductive adhesive layer of acrylate pressure-sensitive adhesive and conductive filler, an insulating layer of fluoropolyimide film and a release film layer by using vinyl di(methoxy)phenylsilane modified in an electromagnetic shielding film is a combination of a conductive adhesive layer of a conductive filler, a fluorine-containing polyimide film and a release film layer. , solve the problem of insufficient shielding performance and adhesive strength of the existing electromagnetic shielding film, and realizes a high-performance and stable electromagnetic shielding protective film.
Patent Information
- Application Number
- CN202211376853.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-11-04
AI Technical Summary
When existing electromagnetic shielding films are used for a long time, there are defects in shielding performance and bonding strength between each layer, which is difficult to meet the needs of high performance and stability.
A structure including a metal foil layer, a first conductive adhesive layer and a second conductive adhesive layer are adopted, wherein the conductive adhesive layer is made of vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive and conductive filler, and the insulating layer is The fluoropolymer film is coated with a microconcave coating, combined with the release film layer to form a high-performance electromagnetic shielding protective film.
It achieves excellent shielding performance and interlayer bonding strength, improves the long-term use stability of the electromagnetic shielding film, and has good high temperature resistance, conductivity and heat dissipation capabilities.
Smart Images

Figure QLYQS_1 
Figure BDA0003927061540000031 
Figure BDA0003927061540000041
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electromagnetic shielding films, and in particular to an electromagnetic shielding protective film. Background Art
[0002] Electromagnetic shielding film is the core material for FPC to achieve electromagnetic shielding and ensure normal operation. The growth of consumer electronics, automotive electronics and other fields has driven the growth of FPC demand, bringing high demand for the quantity and quality of electromagnetic shielding. Electromagnetic shielding is the use of shielding materials to block or attenuate the transmission of electromagnetic energy between the shielded area and the outside world. Electromagnetic shielding utilizes the reflection, absorption and guidance of the shielding body on the electromagnetic energy flow, and is closely related to the charge, current and polarization phenomenon induced on the surface of the shielding structure and inside the shielding body. Electromagnetic waves are generated when electronic components are working, which will have a greater or lesser effect on the electronic components and produce a certain degree of interference. At the same time, electronic components will not only be affected by their own electromagnetic interference, but also by electromagnetic interference from the outside world. If the electromagnetic interference exceeds the tolerance value of the electronic components, it will affect their normal use performance.
[0003] Electromagnetic shielding films are usually composite structures composed of multiple functional films, mainly composed of an insulating layer, a metal layer, and a conductive layer. The insulating layer is used to protect the metal layer from being damaged, the metal layer is mainly used to shield external electromagnetic interference, and the conductive layer is used to conduct charge. With the increasing diversification and complexity of electronic components in electronic equipment, the performance requirements for electromagnetic shielding films are also getting higher and higher. Existing electromagnetic shielding films have certain defects in shielding performance, bonding strength between layers, and other properties when used for a long time. Summary of the invention
[0004] The object of the present invention is to provide an electromagnetic shielding protective film, which has excellent long-term performance stability in terms of both shielding performance and bonding strength between layers, and has a simple structure and is easy to carry out industrial production.
[0005] The embodiments of the present invention are implemented by the following technical solutions:
[0006] An electromagnetic shielding protective film comprises a metal foil layer and a first conductive adhesive layer and a second conductive adhesive layer arranged on both sides of the metal foil layer; an insulating layer is arranged on the side of the first conductive adhesive layer away from the metal foil layer; and a release film layer is arranged on the side of the second conductive adhesive layer away from the metal foil layer;
[0007] The first conductive adhesive layer and the second conductive adhesive layer both include: an organic siloxane-modified acrylate pressure-sensitive adhesive and a conductive filler; the organic siloxane-modified acrylate pressure-sensitive adhesive is a vinyl di(methoxy)phenylsilane-modified acrylate pressure-sensitive adhesive.
[0008] Furthermore, the molecular structure of the vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive is:
[0009]
[0010] In the formula, w=8-35, x=10-30, y=1-5, z=5-50.
[0011] Furthermore, the thickness of the first conductive adhesive layer is 5 μm-45 μm; the thickness of the second conductive adhesive layer is 5 μm-65 μm; and the thickness of the metal foil layer is 0.3 μm-1.5 μm.
[0012] Furthermore, the metal foil layer is one of copper foil, nickel foil, zinc foil and aluminum foil.
[0013] Furthermore, the conductive filler includes reduced graphene oxide and metal oxide.
[0014] Furthermore, the mass ratio of the reduced graphene oxide to the organosiloxane-modified acrylate pressure-sensitive adhesive is 1:5-1:200; the mass ratio of the metal oxide to the organosiloxane-modified acrylate pressure-sensitive adhesive is 1:5-1:200.
[0015] Furthermore, the reduced graphene oxide is a lamellar structure, and the lamellar structure contains one or more of carboxyl, hydroxyl, epoxy, and carbonyl groups; the metal oxide is one or a mixture of several of ferroferric oxide, nickel oxide, zinc oxide, antimony dioxide, tin oxide, and cuprous oxide.
[0016] Furthermore, an insulating layer is provided on a side of the first conductive adhesive layer away from the metal foil layer; and a release film layer is provided on a side of the second conductive adhesive layer away from the metal foil layer.
[0017] Furthermore, the insulating layer is a fluorinated polyimide film, and the volume resistance of the insulating layer is 10 14-16 Ω·cm, thickness is 5μm-50μm;
[0018] The preparation method of the polyimide film is as follows: 2,2-bis[4-(4-amino-2-trifluoroethoxyphenoxy)phenyl]hexafluoropropane and pyromellitic acid dianhydride are prepared by polycondensation, casting, imidization and the like; the molecular structure of the polyimide film is:
[0019]
[0020] Furthermore, the release film layer is a release film with a PET film as a substrate and coated with a silicone release agent; the release film layer has a thickness of 5 μm-100 μm.
[0021] A method for preparing an electromagnetic shielding protective film comprises the following steps: firstly coating a first conductive adhesive layer on an insulating layer, curing it in an oven and then laminating it with a metal foil layer, then coating a second conductive adhesive layer on the metal foil layer, curing it in an oven and then laminating it with a release film layer.
[0022] Specifically, the coating method is micro-concave coating, and the micro-concave roller used is a ceramic micro-concave roller or a metal micro-concave roller with a mesh size of 40 mesh, 45 mesh, 50 mesh, 60 mesh, 70 mesh, and 80 mesh; the lamination pressure of the metal foil layer is 0.15~0.32MPa; the lamination pressure of the release film layer is 0.13~0.26MPa.
[0023] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:
[0024] 1. The conductive adhesive layer of the present invention uses vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive as an adhesive, and this pressure-sensitive adhesive has excellent high temperature resistance; at the same time, the delocalized electrons existing in the conjugated large π bonds in vinyl di(methoxy)phenylsilane are conductive, which can further enhance the conductive ability of the conductive adhesive layer.
[0025] 2. The conductive adhesive layer of the present invention uses reduced graphene oxide and metal oxide as conductive fillers at the same time. The hydrophilic carboxyl, hydroxyl, epoxy, carbonyl and lipophilic carbon hexagonal ring exist in the graphene oxide sheet structure at the same time, so that it can be used as a Pickering emulsifier to improve the dispersibility of the metal oxide in the glue; at the same time, the synergistic conductivity of the two fillers makes the present invention have better conductivity and thus higher shielding effectiveness; in addition, the reduced graphene oxide and the metal oxide of the present invention will also produce a synergistic thermal conductivity effect, so that the heat dissipation capacity of the present invention is higher.
[0026] 3. The present invention adopts a fluorinated polyimide film as an insulating layer, which has a very high dielectric constant, a high breakdown voltage, and good electrical resistance, and also has good flame retardancy. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 A schematic diagram of the structure of the electromagnetic shielding protective film provided in Example 1 of the present invention;
[0029] Icon: 1-insulating layer, 2-first conductive adhesive layer, 3-metal foil layer, 4-second conductive adhesive layer, 5-release film layer. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0031] Example 1
[0032] An electromagnetic shielding protective film, comprising a metal foil layer 3 (nickel foil layer) and a first conductive adhesive layer 2 and a second conductive adhesive layer 4 arranged on both sides of the nickel foil layer; a fluorine-containing polyimide film layer is arranged on the side of the first conductive adhesive layer 2 away from the nickel foil layer; a release film layer 5 is arranged on the side of the second conductive adhesive layer 4 away from the nickel foil layer;
[0033] Among them, the first conductive adhesive layer 2 and the second conductive adhesive layer 4 both include: vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive and conductive filler; the conductive filler is a composite conductive filler doped with reduced graphene oxide and ferroferric oxide; the release film layer 5 is a release film with a PET film as a substrate and coated with an organic silicone release agent; the fluorinated polyimide film layer of the insulating layer 1 is obtained by condensation polymerization, casting, imidization and other processes of 2,2-bis[4-(4-amino-2-trifluoroethoxyphenoxy)phenyl]hexafluoropropane and pyromellitic acid dianhydride, and the volume resistance of the insulating layer 1 reaches 1014-16Ω·cm;
[0034] The specific addition ratio is: the mass ratio of reduced graphene oxide to vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive is 1:100; the metal oxide conductive filler is ferrosoferric oxide, and the mass ratio of ferrosoferric oxide to vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive is 1:150;
[0035] Specifically, the thickness is as follows: the nickel foil layer is 0.5 μm thick, the first conductive adhesive layer 2 is 15 μm thick, the second conductive adhesive layer 4 is 25 μm thick, the insulating layer 1 is 20 μm thick, and the release film layer 5 is 15 μm thick;
[0036] A method for preparing an electromagnetic shielding protective film comprises the following steps: firstly coating a first conductive adhesive layer 2 on an insulating layer 1, laminating a metal foil layer 3 after curing in an oven, then coating a second conductive adhesive layer 4 on the metal foil layer 3, and laminating a release film layer 5 after curing in an oven; the coating method is micro-concave coating, and the micro-concave roller used is a 45-mesh ceramic micro-concave roller; the laminating pressure of the metal foil layer 3 is 0.18 MPa; the laminating pressure of the release film layer 5 is 0.16 MPa; the oven temperature is as shown in Table 1:
[0037] Table 1 Oven temperature
[0038]
[0039] Example 2
[0040] The difference between this embodiment and embodiment 1 is that:
[0041] The metal foil layer is copper foil, and the thickness of the metal foil layer is 0.3 μm;
[0042] The thickness of the first conductive adhesive layer is 10 μm, and the thickness of the second conductive adhesive layer is 15 μm;
[0043] The mass ratio of reduced graphene oxide to vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive is 1:85, the metal oxide conductive filler is ferrosoferric oxide and zinc oxide, the mixed mass ratio is 3:1, and the mass ratio of metal oxide conductive filler to vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive is 1:120;
[0044] The thickness of the insulating layer is 10 μm, the thickness of the release film layer 5 is 25 μm, and the micro-concave roller is a 50-mesh metal micro-concave roller.
[0045] Example 3
[0046] The difference between this embodiment and embodiment 1 is that:
[0047] The metal foil layer is zinc foil, and the thickness of the metal foil layer is 0.4 μm;
[0048] The thickness of the first conductive adhesive layer is 15 μm, and the thickness of the second conductive adhesive layer is 15 μm;
[0049] The mass ratio of reduced graphene oxide to vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive is 1:130, the metal oxide conductive filler is ferrosoferric oxide and antimony dioxide, the mixing mass ratio is 1:1, and the mass ratio of reduced graphene oxide to vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive is 1:180.
[0050] The thickness of the insulating layer 1 is 15 μm, the thickness of the release film layer 5 is 10 μm, and the micro-concave roller is a 60-mesh metal micro-concave roller.
[0051] Comparative Example 1
[0052] The difference between this comparative example and Example 1 is that the pressure-sensitive adhesive used is a conventional acrylic pressure-sensitive adhesive, the conductive filler added is ferrosoferric oxide, and the insulating layer used is a conventional polyimide film without the introduction of fluorine element.
[0053] Comparative Example 2
[0054] The difference between this comparative example and Example 3 is that the added conductive filler is antimony dioxide, and the used insulating layer is a PET film.
[0055] Experimental Example 1
[0056] Relevant performance tests were performed on the electromagnetic shielding protective films prepared in Examples 1-3 and Comparative Examples 1 and 2, and the results are shown in Table 2.
[0057] Table 2 Performance of electromagnetic shielding protective films obtained in Examples and Comparative Examples
[0058]
[0059] It can be seen from the data in Table 2 that the electromagnetic shielding protective film of the present invention has excellent shielding performance, and the conductive adhesive layer of the present invention adopts vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive as an adhesive, which has good high temperature resistance under the synergistic effect and can enhance the conductivity of the adhesive layer; and the present invention adopts fluorinated polyimide film as an insulating layer, and this insulating layer has a very high dielectric constant, a high breakdown voltage, and very good resistivity.
[0060] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An electromagnetic shielding protective film, It is characterized in that It comprises a metal foil layer and a first conductive adhesive layer and a second conductive adhesive layer arranged on both sides of the metal foil layer; The first conductive adhesive layer and the second conductive adhesive layer both include: vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive, reduced graphene oxide and metal oxide; The molecular structure of the vinyl di(methoxy)phenylsilane modified acrylate pressure-sensitive adhesive is: , Where w=8-35, x=10-30, y=1-5, z=5-50; The metal oxide is one or a mixture of ferroferric oxide, nickel oxide, zinc oxide, antimony dioxide, tin oxide, and cuprous oxide; An insulating layer is provided on the side of the first conductive adhesive layer away from the metal foil layer; the insulating layer is a fluorinated polyimide film, and the volume resistance of the insulating layer is 10 14-16 Ω·cm.
2. The electromagnetic shielding protective film according to claim 1, It is characterized in that The thickness of the first conductive adhesive layer is 5 μm-45 μm; the thickness of the second conductive adhesive layer is 5 μm-65 μm; and the thickness of the metal foil layer is 0.3 μm-1.5 μm.
3. The electromagnetic shielding protective film according to claim 1, It is characterized in that The mass ratio of the reduced graphene oxide to the organosiloxane-modified acrylate pressure-sensitive adhesive is 1:5-1:200; the mass ratio of the metal oxide to the organosiloxane-modified acrylate pressure-sensitive adhesive is 1:5-1:
200.
4. The electromagnetic shielding protective film according to claim 3, It is characterized in that The reduced graphene oxide is a sheet structure, and the sheet structure contains hydrophilic groups and lipophilic groups.
5. The electromagnetic shielding protective film according to claim 1, It is characterized in that A release film layer is disposed on a side of the second conductive adhesive layer away from the metal foil layer.
6. The electromagnetic shielding protective film according to claim 5, It is characterized in that The thickness of the insulating layer is 5 μm-50 μm.
7. The electromagnetic shielding protective film according to claim 5, It is characterized in that The release film layer is a release film with a PET film as a base material and coated with an organic silicon release agent; the thickness of the release film layer is 5 μm-100 μm.