A polyolefin elastomer composition for photovoltaic encapsulation film
By optimizing the structure and ratio of ethylene and long-chain α-olefin copolymers, a polyolefin elastomer composition with high light transmittance and water vapor isolation ability was prepared, which solved the problems of breathability and durability of photovoltaic packaging materials and achieved for more efficient photovoltaic packaging performance.
Patent Information
- Application Number
- CN202211464156.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-11-22
AI Technical Summary
Existing photovoltaic packaging materials have problems such as poor air permeability, intolerance to UV light, and easy yellowing and shedding, which lead to reduced battery life and efficiency. Existing patents fail to provide in-depth analysis of the relationship between polymer structure and performance.
By optimizing the α-insertion rate, molecular weight, melting point and glass transition temperature of ethylene and long-chain α-olefin copolymer, combined with the ratio of ethylene and vinyl carboxylate copolymer and free radical initiator, it was prepared by continuous solution polymerization. The polyolefin elastomer composition ensures that its light transmittance, water vapor transmittance and volume resistivity are at high levels.
The excellent performance of the polyolefin elastomer composition is achieved, the light transmittance, water vapor isolation ability and anti-aging performance of the photovoltaic packaging film are improved, it can adapt to various extreme conditions and extend the service life.
Smart Images

Figure BDA0003956775350000021 
Figure BDA0003956775350000031 
Figure BDA0003956775350000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyolefins, and in particular to a polyolefin elastomer composition for photovoltaic encapsulation films. Background Art
[0002] With the vigorous development of the photovoltaic industry, the service life and stability of photovoltaic products have become issues of increasing market concern. As the core components of photovoltaic products, the service life and efficiency of solar panels have become extremely important, and the requirements for battery packaging materials have become increasingly higher. The poor water and oxygen isolation effect of packaging materials has led to a reduction in battery life. The decrease in light transmittance caused by packaging materials has affected the photoelectric conversion efficiency and the poor PID resistance of materials are the core problems encountered by battery packaging materials.
[0003] Polyethylene vinyl acetate material has excellent melt fluidity and low processing temperature. The optical properties and adhesion of the film after formula casting can well meet the requirements of photovoltaic encapsulation film; coupled with low cost, it has occupied more than 80% of the photovoltaic encapsulation film market in the past 30 years. However, its inherent defects such as poor air permeability and UV resistance, easy yellowing and shedding limit its development. What is more fatal is that polyvinyl acetate material is easily hydrolyzed to produce acetic acid, resulting in potential induced decay, making it difficult to continue to be used in large-scale photovoltaic power stations. Polyolefin (POE) is increasingly attracting attention from the photovoltaic industry for its low water vapor transmission rate, high volume resistivity, high light transmittance, high insulation strength and good PID resistance.
[0004] Existing patents involve the preparation technology of POE encapsulation film or the improvement of a certain performance of it as an encapsulation material. For example, the Chinese patent with publication number CN110809602A discloses a polyolefin composition for photovoltaic encapsulation film, which shortens the processing time of forming the encapsulation film; the Chinese patent with application number 2018106435804 provides a preparation method of silane-grafted POE photovoltaic encapsulation film with low encapsulation defective rate and high assembly production efficiency; the Chinese patent with application number 201610668040.2 discloses a composite crosslinking agent for POE encapsulation film and its application, which adopts a three-component composite crosslinking agent, so that the prepared POE encapsulation film has both the stability of cast film process and the high-efficiency crosslinking property of lamination curing.
[0005] The above patents have not been able to analyze the relationship between the structure of the polymer itself and its performance. They have only optimized the processing and preparation methods of the polymer, or involved a formula that can improve a certain performance, but have not been able to fundamentally find the decisive role of the sequence structure in the ethylene-α-olefin copolymer on the polymer performance, let alone its application in the POE+EVA encapsulation film composition for photovoltaics. Summary of the invention
[0006] The technical problem solved by the present invention is to provide a polyolefin elastomer composition for photovoltaic encapsulation film, whose light transmittance, water vapor permeability, volume resistivity and other properties are maintained at a relatively high level.
[0007] In view of this, the present application provides a polyolefin elastomer composition for photovoltaic encapsulation film, comprising:
[0008]
[0009] Preferably, the copolymer of ethylene and long-chain α-olefin has an α-olefin insertion rate of 8.0 to 26.0 mol%, a melt mass flow index of 0.2 g / 10 min to 115.0 g / 10 min, a melting point of 50 to 85°C, a crystallization temperature of 25 to 70°C, a glass transition temperature of -65 to -45°C, and a weight-average molecular weight of 120,000 to 400,000.
[0010] Preferably, the α-olefin in the copolymer of ethylene and long-chain α-olefin is selected from one or more of 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene and 1-decene.
[0011] Preferably, the copolymer of ethylene and long-chain α-olefin is obtained by continuous solution polymerization.
[0012] Preferably, the free radical initiator is selected from dibenzoyl peroxide.
[0013] Preferably, the organosilicon compound is selected from methacryloxysilane.
[0014] Preferably, the content of the copolymer of ethylene and long-chain α-olefin is 75-85 wt%.
[0015] Preferably, the content of the ethylene and vinyl carboxylate copolymer is 10 to 25 wt%.
[0016] Preferably, the content of the free radical initiator is 0.5-1.8 wt %.
[0017] Preferably, the content of the organosilicon compound is 0.5-2.5 wt %.
[0018] The present application provides a polyolefin elastomer composition for photovoltaic encapsulation film, which includes a copolymer of ethylene and a long-chain α-olefin (POE), a copolymer of ethylene and carboxylic ethylene acid (EVA), a free radical initiator and an organosilicon compound; the polyolefin elastomer composition provided in the present application analyzes the α-insertion rate, different molecular weights, different melting points, crystallization temperatures and different melt mass flow indices of POE, and finds the relationship between the POE structure and the performance of the polyolefin elastomer composition, thereby ensuring that the light transmittance, water vapor permeability, volume resistivity and other properties of the polyolefin elastomer composition are maintained at a high level. DETAILED DESCRIPTION
[0019] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0020] The embodiment of the present invention discloses a polyolefin elastomer composition for photovoltaic encapsulation film, comprising:
[0021]
[0022] In the present application, the ethylene-long-chain α-olefin copolymer (POE) has an α-olefin insertion rate of 8.0-26.0 mol%, a melt mass flow index of 0.2 g / 10 min-115.0 g / 10 min, a melting point of 50-85 ° C, a crystallization temperature of 25-70 ° C, a glass transition temperature of -65--45 ° C, and a weight-average molecular weight of 120,000-400,000; the POE with the above characteristics is applied to the polyolefin elastomer composition of the photovoltaic encapsulation film to make it have excellent performance. The content of the POE is 70-90 wt%, specifically, the content of the POE is 75-85 wt%.
[0023] In the POE of the present application, the α-olefin is selected from one or more of 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene and 1-decene; the POE is obtained by continuous solution polymerization; more specifically, ethylene and long-chain α-olefins are subjected to high-temperature solution polymerization under the action of a main catalyst and a co-catalyst to obtain a polyolefin elastomer;
[0024] The main catalyst has a structure as shown in formula (I);
[0025]
[0026] Wherein, R1 is selected from substituted or unsubstituted C1-C10 alkyl, substituted or unsubstituted C6-C15 aryl, and C6-C15 condensed ring containing N;
[0027] R2 is selected from substituted or unsubstituted C1-C10 alkyl;
[0028] X is halogen, alkyl or aryl;
[0029] M is a fourth subgroup transition metal element.
[0030] The main catalyst of the present application forms different compounds when R1, R2, X and M take different substituents. In a specific embodiment, the main catalyst is specifically selected from the following structures:
[0031] N1: R1 = tert-butyl, R2 = methyl, M = Zr, X = methyl;
[0032] N2: R1 = tert-butyl, R2 = tert-butyl, M = Zr, X = methyl;
[0033] N3: R1 = cumyl, R2 = tert-butyl, M = Zr, X = methyl;
[0034] N4: R1 = trityl, R2 = tert-butyl, M = Zr, X = methyl;
[0035] N5: R1 = 3,5-di-tert-butyl, R2 = tert-butyl, M = Zr, X = methyl;
[0036] N6: R1 = 3,5-di-tert-butyl, R2 = methyl, M = Zr, X = methyl;
[0037] N7: R1 = carbazolyl, R2 = methyl, M = Zr,, X = methyl;
[0038] N8: R1 = carbazolyl, R2 = tert-butyl, M = Zr, X = methyl;
[0039] N9: R1 = 3,5-di-tert-butyl, R2 = tert-butyl, M = Hf, X = methyl;
[0040] N10: R1 = carbazolyl, R2 = tert-butyl, M = Hf, X = methyl.
[0041] The co-catalyst described in the present application is specifically selected from one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, methylaluminoxane (MAO), modified methylaluminoxane (MMAO), perfluorophenylboron, triphenylcarbon tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate and N,N-di(hexadecyl)anilinium tetrakis(pentafluorophenyl)borate.
[0042] In the present application, the molar ratio of the co-catalyst to the main catalyst is 150:1 to 3000:1, specifically, the molar ratio of the co-catalyst to the main catalyst is 300:1 to 1000:1; the molar ratio of the above co-catalyst to the main catalyst is calculated based on the molar ratio of the metal elements therein.
[0043] In the present application, the α-olefin is selected from one or more of 1-butene, 1-hexene, 1-octene and 1-decene.
[0044] In the process of preparing the polyolefin elastomer, the polymerization temperature is 100-150° C., the polymerization pressure is 1-5 MPa; more specifically, the polymerization temperature is 130-140° C., the polymerization pressure is 3-4 MPa. The molar ratio of the α-olefin to the ethylene is (2-15):1; more specifically, the molar ratio of the α-olefin to the ethylene is (2-10):1.
[0045] In the polyolefin elastomer composition, the content of the ethylene and carboxylic acid vinyl ester copolymer is 5.0-30.0wt%, specifically, the content of the ethylene and carboxylic acid vinyl ester copolymer is 10-25wt%. If the content of the ethylene and carboxylic acid vinyl ester copolymer is too high, the water vapor transmission rate, aging resistance and anti-potential induction performance of the composition will be significantly reduced.
[0046] The free radical initiator is selected from dibenzoyl peroxide; its content is 0.01-2.0wt%, specifically, the content of the free radical initiator is 0.5-1.8wt%. The organosilicon compound is selected from methacryloxysilane; its content is 0.01-3.0wt%, specifically, the content of the organosilicon compound is 0.5-2.5wt%. If the content of the free radical initiator and the organosilicon compound is too much, the light transmittance of the product will be affected.
[0047] This application conducts in-depth research on ethylene-alpha olefin copolymers with different structures and properties, and blends them with EVA to obtain photovoltaic encapsulation film materials with excellent performance. Compared with existing photovoltaic POE products, while maintaining the properties of POE such as transmittance and volume resistivity at a good level, the product's insertion rate molecular weight, melt index, melting point, crystallization temperature and other indicators are within a wider range, which can be better processed and formed in the actual application process, has better adaptability to various extreme conditions, and has more superior performance and higher application value.
[0048] In order to further understand the present invention, the polyolefin elastomer composition for photovoltaic encapsulation film provided by the present invention is described in detail below in conjunction with examples, and the protection scope of the present invention is not limited by the following examples.
[0049] Example 1
[0050] Ethylene and long-chain α-olefins are subjected to high-temperature solution polymerization under the action of a main catalyst and a co-catalyst to obtain a polyolefin elastomer; the raw materials and reaction conditions involved in the process are specifically shown in Table 1, and the properties of the prepared polyolefin elastomer are specifically shown in Table 2;
[0051] Table 1 Raw materials and parameter data for the preparation of polyolefin elastomers
[0052]
[0053] Table 2 Performance data of different polyolefin elastomers
[0054]
[0055]
[0056] As shown in Table 2, the insertion rate of the above 7 polymers is up to 25.21% (No. 7), but its melting point, crystallization temperature and Tg are the lowest among all combinations, which are 51.56℃, 27.11℃ and -62.56℃ respectively. This is mainly because the insertion of the long side chain of octene will increase the intermolecular distance, increase the side chain movement of the polymer molecules, affect the regularity of the molecular arrangement, and cause the crystallization wafer to become thinner and the crystallinity to become worse. Therefore, the more octene is inserted, the greater the damage to the ethylene crystal segment, the worse the crystallinity of the polymer, and its melting temperature, crystallization temperature and glass transition temperature decrease accordingly. Polymers with poor crystallinity have good light transmittance, which can effectively improve the light transmittance in the application of photovoltaic encapsulation film; and the worse the crystallinity, the lower the glass transition temperature, and the product can still maintain good mechanical properties at lower temperatures, that is, the product can better adapt to extremely complex environments such as low temperature, and can effectively improve the service life of the product in practical applications. Its molecular weight is 214,200, PDI is 2.99, melt mass flow index is 12.29g / 10min, and it is easy to process and shape.
[0057] The minimum insertion rate can reach 8.28%, the molecular weight is 388,000, the PDI is 4.32, and the melt mass flow index is 0.22g / 10min. At this time, the product has poor fluidity and is easier to process and shape. The melting point, crystallization temperature and glass transition temperature of the product are 74.84℃, 62.68℃ and -49.69℃ respectively. This shows that as the amount of octene insertion decreases, the crystallinity of the polymer is better, and the melting point and crystallization temperature of the product are higher.
[0058] In addition, a polymer (No. 5) with a melt mass flow index of 114.96 g / 10 min was obtained, with an α-octene insertion rate of 24.48%, a molecular weight of 125,700, and a molecular weight distribution of 2.56. At this time, the melting point, crystallization temperature and glass transition temperature of this polymer are 54.42°C, 31.10°C and -62.56°C, respectively. This small molecular weight and high insertion rate polymer also has a low crystallinity but is not easy to process. Compared with the No. 7 polymer with similar performance, its molecular weight and insertion rate are significantly lower, which is mainly determined by the difference in its sequence structure. According to nuclear magnetic resonance analysis, compared with the other 6 polymers, the proportion of EEOEOEE sequence in No. 5 polymer is relatively high, which means that the inserted octene sequence is more evenly arranged. Then the crystallinity of the polymer is lower, and the melting point, crystallization temperature and other indicators are reduced accordingly. The large melt mass flow index of the polymer is due to its smaller molecular weight.
[0059] For polymers with insertion rates of 11.27%, 12%, 14.38% and 15.37%, their melting points are 67.71°C, 65.56°C, 62.13°C and 61.13°C, their crystallization temperatures are 49.99°C, 48.17°C, 44.70°C and 40.88°C, and their glass transition temperatures are -51.98°C, -52.58°C, -53.37°C and -53.71°C. With the increase of α-olefin insertion rate, the ethylene crystal segment of the polymer is destroyed, the crystallinity of the polymer deteriorates, the melting point, crystallization temperature and glass transition temperature decrease accordingly, and the light transmittance of the polymer improves. The molecular weights of the polymers are 360,800, 335,200, 222,100 and 176,300 respectively. As the polymerization proceeds, the inserted α-olefin side chains form steric hindrance, which will make the insertion of octene more and more difficult. Therefore, the molecular weight of the polymer tends to show a negative correlation with the insertion rate of α-olefins. The melt index of several polymers is 0.5g / 10min, 0.55g / 10min, 14.28g / 10min and 4.70g / 10min respectively. The melt fluidity of the polymer mainly depends on its molecular weight. The larger the molecular weight, the worse the polymer fluidity. Therefore, reasonable control of the molecular weight during the polymerization process can ensure the processing performance of the polymer product.
[0060] Example 2
[0061] The compositions obtained by mixing the No. 7 ethylene-1-octene copolymer in Example 1 with ethylene-vinyl acetate, a free radical initiator, and an organosilicon compound in different proportions were made into sheets, and their tensile properties, light transmittance, volume resistivity, etc. were characterized respectively. The results are shown in Tables 5 and 6; the contents of the compositions of different components are shown in Tables 3 and 4;
[0062] Table 3 Composition data of different polyolefin elastomer compositions
[0063] a b c d e f g Ethylene-1-octene copolymer (%) 75 85 90 76 77 76 77 Ethylene-vinyl acetate copolymer (%) 20 10 5 20 20 20 20 Free radical initiator (%) 2 2 2 2 2 1 1 Organic silicon compound (%) 3 3 3 2 1 3 2
[0064] Table 4 Composition data of different polyolefin elastomer compositions (continued from Table 1)
[0065] h i j k l m n Ethylene-1-octene copolymer (%) 76.5 77.5 70 70 70 70 90 Ethylene-vinyl acetate copolymer (%) 20 20 25 29 27 29.98 9.8 Free radical initiator (%) 0.5 0.5 2 0.5 2 0.01 0.01 Organic silicon compound (%) 3 2 3 0.5 1 0.01 0.01
[0066] Table 5 Performance data of different polyolefin elastomer compositions
[0067] a b c d e f g Tensile elongation at break (%) 960 1050 1120 1400 1380 1501 1680 Light transmittance (%) 70.1 75.0 82.3 73.6 74.8 73.4 78.2 <![CDATA[Volume resistivity × 10 15 > 0.88 1.02 2.43 1.25 2.55 1.67 3.60 Water vapor transmission rate (%) 3.0 3.9 4.4 3.5 4.0 4.2 5.0
[0068] Table 6 Performance data of different polyolefin elastomer compositions (continued from Table 1)
[0069] h i j k l m n Tensile elongation at break (%) 960 1050 1120 1400 1380 1501 1680 Light transmittance (%) 70.1 77.2 70.1 71.6 71.8 70.4 88.1 <![CDATA[Volume resistivity × 10 15 > 0.88 1.02 2.43 1.25 2.55 1.67 3.60 Water vapor transmission rate (%) 3.0 3.2 3.2 3.5 3.3 2.9 5.0
[0070] The results show that the above 14 olefin polymer product compositions have excellent tensile properties, light transmittance and low volume resistivity; they can all be used as high-performance photovoltaic encapsulation films in the photovoltaic field.
[0071] In summary, the above series of ethylene-α-olefin copolymers with different α-olefin insertion amounts, different molecular weights, and different crystallization properties were studied, and polymers that are more suitable for certain extreme environments or application scenarios can be selected as needed; and the correlation between structure and performance was obtained by analyzing their structure and performance, and finally several polymers were obtained with excellent photovoltaic performance, which provides a reference for the design and application development of more ethylene-α-olefin polymers.
[0072] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0073] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A polyolefin elastomer composition for photovoltaic encapsulation film, comprising: The copolymer of ethylene and long-chain α-olefin has an α-olefin insertion rate of 8.0 to 26.0 mol%, a melt mass flow index of 0.2 g / 10 min to 115.0 g / 10 min, a melting point of 50 to 85° C., a crystallization temperature of 25 to 70° C., a glass transition temperature of -65 to -45° C., and a weight average molecular weight of 120,000 to 400,000.
2. The polyolefin elastomer composition according to claim 1, characterized in that The α-olefin in the copolymer of ethylene and long-chain α-olefin is selected from one or more of 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene and 1-decene.
3. The polyolefin elastomer composition according to claim 1, characterized in that The copolymer of ethylene and long-chain alpha-olefin is obtained by continuous solution polymerization.
4. The polyolefin elastomer composition according to claim 1, characterized in that The free radical initiator is selected from dibenzoyl peroxide.
5. The polyolefin elastomer composition according to claim 1, characterized in that The organosilicon compound is selected from methacryloxysilane.