A device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization and its use method

Through pulse current rapid heating spheroidization technology, the problems of slow heating and severe oxidation in the preparation of high-entropy alloy semi-solid billets are solved, and the efficient preparation of fine-grained multi-level structure semi-solid billets is achieved, which improves billet quality and processing efficiency.

CN115747428BActive Publication Date: 2024-10-11HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211558729.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-10-11
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

During the preparation process of high-entropy alloy semi-solid billets, the heating temperature rises slowly and the isothermal spheroidization time is long, resulting in low preparation efficiency, strict process parameter control and serious oxidation problems.

Method used

Pulse current rapid heating spheroidization technology is used, and a device composed of a hydraulic loading cylinder and a pulse DC power supply is used to achieve rapid heating and isothermal treatment of high-entropy alloy semi-solid billets to reduce the risk of oxidation.

Benefits of technology

The preparation efficiency of semi-solid blanks is significantly improved, the coarsening of solid grains is avoided, the degree of oxidation is reduced, a finer multi-level structure microstructure and higher quality semi-solid blanks are obtained, and energy consumption and costs are saved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115747428B_ABST
    Figure CN115747428B_ABST
Patent Text Reader

Abstract

A device for preparing a multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization and a method for using the same relate to a device for preparing a multi-level structure fine-grained high-entropy alloy semi-solid billet and a method for using the same. The present invention aims to solve the technical problems of slow heating and heating in the current preparation process of high-entropy alloy semi-solid billets, long time-consuming semi-solid isothermal spheroidization process, grain coarsening in the semi-solid isothermal treatment process, and severe oxidation in the preparation process of semi-solid billets. The present invention improves the efficiency of preparing high-entropy alloy semi-solid billets by rapid pulse current heating and rapid spheroidization of powder metallurgy preset structures, thereby reducing the degree of oxidation in the preparation process of high-entropy alloy semi-solid billets; due to rapid heating and rapid semi-solid isothermal, the excellent spheroidization effect of the semi-solid microstructure is met, the coarsening of solid phase grains is avoided, and a semi-solid microstructure with finer grains can be obtained, and at the same time, a finer amplitude modulation decomposition multi-level structure is formed in the solid phase grains.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a device for preparing a multi-level structure fine-grained high-entropy alloy semi-solid blank and a use method thereof. Background Art

[0002] High entropy alloys have a series of excellent properties such as high strength, resistance to high temperature softening, corrosion resistance, high temperature oxidation resistance and radiation resistance. They are the ideal materials for the new generation of extreme environments. In order to realize the application of high entropy alloys, the processing and manufacturing of high entropy alloys are the challenges that need to be faced urgently. Semi-solid processing technology has low forming loads and excellent thixotropic flow filling ability. It is an ideal processing and manufacturing method for high-strength and low-plasticity high entropy alloys. So far, many high entropy alloys have been proven to have a wide semi-solid range, which is very suitable for semi-solid processing.

[0003] In semi-solid processing, the preparation of semi-solid billets is the most core link of this technology. The preparation of semi-solid billets usually requires a semi-solid isothermal heat treatment process to form a semi-solid microstructure with a liquid film wrapping a nearly spherical solid phase grain. Generally speaking, semi-solid billets with a high degree of spheroidization and a small solid phase grain size have better thixoforming properties and better mechanical properties after semi-solid processing. Therefore, the degree of spheroidization and grain size of the solid phase grains need to be strictly controlled during the isothermal heat treatment process. The semi-solid high entropy alloy billets reported so far are all spheroidized by recrystallization of the deformed structure of the ingot and subsequent semi-solid isothermal remelting process. The isothermal spheroidization process requires a relatively long kinetic time, and the isothermal heat treatment time is usually in the range of several minutes to tens of minutes. Severely deformed microstructures (such as rolled and extruded microstructures) require a longer processing time to complete the spheroidization process. In addition, the heating of semi-solid billets is usually carried out by radiation heat transfer using a resistance furnace, and the heating efficiency is low (usually the heating rate is 10-20℃ / min). The above-mentioned traditional semi-solid billet preparation method is time-consuming and requires strict control of spheroidization and avoidance of grain growth, which limits the efficiency of semi-solid processing. On the other hand, the oxidation reaction of the alloy in the semi-solid range is often very violent. Long-term heating and semi-solid isothermal treatment causes severe oxidation of the semi-solid billet. If inert gas protection is used, the billet preparation cost will inevitably increase.

[0004] Therefore, improving the heating efficiency and shortening the isothermal spheroidization time in the semi-solid billet preparation process are the key to improving the preparation efficiency of high-entropy alloy semi-solid billets. At the same time, fine-grained semi-solid structure can be obtained and the degree of billet oxidation can be greatly reduced. It has many benefits for optimizing the preparation process of high-entropy alloy semi-solid billets and improving the properties of alloys after semi-solid processing. Summary of the invention

[0005] The present invention aims to solve the technical problems of slow heating and slow temperature rise in the current preparation process of high entropy alloy semi-solid billet, long time-consuming semi-solid isothermal spheroidization process, low semi-solid billet preparation efficiency, strict control of isothermal process process parameters, grain coarsening in the semi-solid isothermal treatment process and severe oxidation in the preparation process of semi-solid billet, and provide a pulse current rapid heating and spheroidization device for preparing multi-level structure fine-grained high entropy alloy semi-solid billet and a method for using the same.

[0006] The pulse current rapid heating spheroidization device for preparing a multi-level structure fine-grained high-entropy alloy semi-solid billet of the present invention comprises a hydraulic loading cylinder (1), an upper support plate (2), a support column (3), an adjustment support block (4), a support block insulating mica plate (5), an upper movable chuck (6), a pressure head pressure plate (7), an upper electrode pressure head (8), a pressure head fixing bolt (9), an electrode pressure head fixing wedge block (10), a chuck insulating mica plate (11), a solder resist tantalum sheet (12), a billet (13), a lower electrode pressure head (14), a lower fixed chuck (15), a moving wheel (16), a chuck pad (17), a lower support plate (18), a pulsed DC power supply (19), a thermocouple (20) and a force sensor (21);

[0007] The hydraulic loading cylinder (1) is fixed on the upper surface of the upper support plate (2), and the piston rod (1-1) of the hydraulic loading cylinder (1) passes through the upper support plate (2) and is slidably connected to the upper support plate (2), and the bottom surface of the piston rod (1-1) is fixedly connected to the upper surface of the upper movable chuck (6); the upper movable chuck (6) is arranged below the upper support plate (2), and a groove (6-1) is arranged between two opposite side walls of the movable chuck (6), and the two opposite inner walls of the groove (6-1) are inclined surfaces, and the groove ( 6-1) opens vertically downward and the opening of the groove (6-1) gradually becomes smaller as it goes downward; the two opposite side walls of the electrode pressure head fixing wedge block (10) respectively match the two opposite inner walls of the groove (6-1); the upper surface of the electrode pressure head fixing wedge block (10) is a plane; a stepped hole is arranged at the center of the electrode pressure head fixing wedge block (10); the electrode pressure head fixing wedge block (10) is arranged in the groove (6-1) and is wedged into the lower end of the groove (6-1) through the matching inclined surfaces; and a A clamping head insulating mica plate (11) is clamped between the electrode pressure head fixing wedge block (10) and the groove (6-1) to prevent the pulse current from passing through the upper movable clamp (6); the upper electrode pressure head (8) is arranged in the stepped hole of the electrode pressure head fixing wedge block (10), a pressure head pressing plate (7) is arranged on the upper surface of the upper electrode pressure head (8), and a plurality of pressure head fixing bolts (9) are arranged between the upper surface of the pressure head pressing plate (7) and the lower surface of the electrode pressure head fixing wedge block (10) to fix the upper electrode pressure head (8) ) is fixed in the stepped hole of the electrode pressure head fixed wedge block (10); a support block insulating mica plate (5) is placed on the upper surface of the pressure head pressure plate (7), and an adjustment support block (4) is arranged on the upper surface of the support block insulating mica plate (5). The adjustment support block (4) is tightly clamped between the upper surface of the groove (6-1) and the support block insulating mica plate (5). The support block insulating mica plate (5) is to prevent the pulse current from passing through the adjustment support block (4) and the upper movable clamp (6) and the hydraulic loading cylinder (1) connected to the adjustment support block (4);

[0008] The lower fixed chuck (15) and the components therein are arranged in the same manner and in the same size as the upper movable chuck (6). The lower fixed chuck (15) is arranged directly below the upper movable chuck (6). The groove of the lower fixed chuck (15) opens vertically upward and corresponds to the position of the groove (6-1) of the upper movable chuck (6). The lower fixed chuck (15) and the upper movable chuck (6) are arranged symmetrically along a horizontal plane. The blank (13) is arranged between the upper electrode pressing head (8) and the lower electrode pressing head (14). The upper surface and the lower surface of the blank (13) are both planes and each is provided with a solder resist tantalum sheet (12). The function of the solder resist tantalum sheet (12) is to prevent the blank (13) from being welded with the upper electrode pressure head (8) and the lower electrode pressure head (14) during the heating and heat preservation process; the lower fixed clamp (15) is fixed to the lower support plate (18) through the clamp pad (17), and the lower support plate (18) is located below the lower fixed clamp (15) and the clamp pad (17); two support columns (3) are symmetrically fixed between the lower support plate (18) and the upper support plate (2), and a plurality of moving wheels (16) are evenly arranged below the lower support plate (18), and the moving wheels (16) facilitate the device to move to the vicinity of the forming equipment;

[0009] The two poles of the pulsed DC power supply (19) are respectively connected to the upper electrode pressing head (8) and the lower electrode pressing head (14); the pulsed DC power supply (19), the upper electrode pressing head (8), two tantalum solder resist sheets (12), the blank (13) and the lower electrode pressing head (14) form a current closed loop; the blank (13) is connected to the thermocouple (20); and the force sensor (21) is connected to the hydraulic loading cylinder (1).

[0010] The method for using the pulse current rapid heating spheroidization device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet of the present invention is as follows:

[0011] Step 1: cutting a blank (13) of a desired size from a high entropy alloy block sintered by powder metallurgy, wherein the blank (13) has two opposite end surfaces parallel to each other;

[0012] Step 2: grinding the surface oxide scale of the cut blank (13) to ensure good electrical conductivity;

[0013] Step 3: Welding a temperature monitoring thermocouple (20) onto the blank (13), placing a solder resist tantalum sheet (12) on the upper end surface of the lower electrode pressure head (14), and then placing the blank (13) connected with the thermocouple, and then placing another solder resist tantalum sheet (12) on the upper surface of the blank (13);

[0014] Step 4: The hydraulic loading cylinder (1) drives the upper movable chuck (6) and the upper electrode pressing head (8) to move downward together, so that the lower end surface of the upper electrode pressing head (8) contacts the solder resist tantalum sheet (12) on the upper surface of the blank (13), and applies a clamping load, the maximum load F does not exceed 5S, the unit is N, and the S is the area of ​​the lower surface of the upper electrode pressing head (8), the unit is mm 2 , to prevent the blank (13) from deforming at high temperatures;

[0015] Step 5: starting the pulsed DC power supply (19) to heat the blank (13) at a heating rate of 10°C / s to 30°C / s; using a thermocouple (20) to monitor the temperature of the blank (13) during the heating process;

[0016] Step 6: After the blank (13) is heated to a semi-solid temperature of 1175°C to 1225°C, the temperature is maintained isothermally for 5s to 20s;

[0017] Step 7: Turn off the pulse DC power supply (19), and the hydraulic loading cylinder (1) drives the upper movable chuck (6) and the upper electrode pressing head (8) to move upward together;

[0018] Step 8: Use a clamp to remove the blank (13), and immediately transfer it to room temperature water for cooling to obtain a semi-solid blank.

[0019] In the present invention, a hydraulic loading cylinder (1) is used to drive an upper movable chuck (6) and an upper electrode pressing head (8) to move downward together, and the hydraulic loading cylinder (1) applies a clamping load to achieve good contact between the upper electrode pressing head (8) and the lower electrode pressing head (14) and the solder resist tantalum sheet (12) and the blank (13); the applied clamping load is monitored by a force sensor (21); the blank (13) is heated by the current Joule heating effect generated by the pulse current of a pulsed DC power supply (19); and the temperature of the blank (13) is monitored by a thermocouple (20).

[0020] The device and method of the present invention are suitable for preparing multi-level structure fine-grained semi-solid billets of high entropy alloys sintered by powder metallurgy such as Al-Co-Cr-Cu-Fe-Ni, Al-Fe-Cr-Cu-Ni, Al-Co-Cr-Cu-Fe and Cr-Cu-Fe-Mn-Ni.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention uses rapid pulse current heating and rapid spheroidization of powder metallurgy preset structures. The billet heating process only takes 40s to 120s (step five), and the semi-solid insulation time only takes 5s to 20s (step six), which greatly improves the efficiency of preparing high-entropy alloy semi-solid billets.

[0023] 2. In the present invention, due to rapid heating and rapid semi-solid isothermal treatment, the coarsening of solid phase grains is avoided while satisfying the excellent spheroidization effect of the semi-solid microstructure. Compared with the traditional method, a semi-solid microstructure with finer grains can be obtained, and a finer amplitude modulation decomposition multi-level structure is formed in the solid phase grains.

[0024] 3. The present invention significantly reduces the degree of oxidation in the preparation process of the semi-solid billet of the high entropy alloy, and improves the quality of the semi-solid billet; the preparation process does not require inert gas protection, which saves costs;

[0025] 4. This method has low energy consumption in the process of preparing high entropy alloy semi-solid billet and has better energy-saving effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of a device for preparing a multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization according to a specific embodiment of the first embodiment;

[0027] Figure 2 for Figure 1 A magnified schematic diagram of the middle area A;

[0028] Figure 3 The Al sintered by powder metallurgy in step 1 of experiment 1 0.8 Co 0.5 Cr 1.5 Original microstructure of CuFeNi high entropy alloy billet;

[0029] Figure 4 Al obtained in step 8 of experiment 1 0.8 Co 0.5 Cr 1.5 The microstructure of the CuFeNi semi-solid billet was taken by scanning electron microscope (SEM) at low magnification;

[0030] Figure 5 Al obtained in step 8 of experiment 1 0.8 Co 0.5 Cr 1.5 The microstructure of the CuFeNi semi-solid billet taken by scanning electron microscope (SEM) at high magnification;

[0031] Figure 6 Al obtained in step 8 of experiment 1 0.8 Co 0.5 Cr 1.5 Microstructure of CuFeNi semi-solid billet taken by transmission electron microscope (TEM);

[0032] Figure 7 Al obtained in step 8 of experiment 1 0.8 Co0.5 Cr 1.5 Oxidation weight gain diagram of CuFeNi semi-solid billet under short-time holding. DETAILED DESCRIPTION

[0033] Specific implementation method 1: This implementation method is a device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization, such as Figure 1 and Figure 2 As shown, it specifically consists of a hydraulic loading cylinder (1), an upper support plate (2), a support column (3), an adjustment support block (4), a support block insulating mica plate (5), an upper movable chuck (6), a pressure head pressure plate (7), an upper electrode pressure head (8), a pressure head fixing bolt (9), an electrode pressure head fixing wedge (10), a chuck insulating mica plate (11), a solder resist tantalum sheet (12), a blank (13), a lower electrode pressure head (14), a lower fixed chuck (15), a moving wheel (16), a chuck pad (17), a lower support plate (18), a pulsed DC power supply (19), a thermocouple (20) and a force sensor (21);

[0034] The hydraulic loading cylinder (1) is fixed on the upper surface of the upper support plate (2), and the piston rod (1-1) of the hydraulic loading cylinder (1) passes through the upper support plate (2) and is slidably connected to the upper support plate (2), and the bottom surface of the piston rod (1-1) is fixedly connected to the upper surface of the upper movable chuck (6); the upper movable chuck (6) is arranged below the upper support plate (2), and a groove (6-1) is arranged between two opposite side walls of the movable chuck (6), and the two opposite inner walls in the groove (6-1) are inclined surfaces, and the opening of the groove (6-1) is vertically downward and the opening of the groove (6-1) gradually becomes smaller as it goes downward; the two opposite side walls in the electrode pressure head fixed wedge block (10) respectively match the two opposite inner walls in the groove (6-1), the upper surface of the electrode pressure head fixed wedge block (10) is a plane, and a stepped hole is arranged at the center of the electrode pressure head fixed wedge block (10), and the electrode pressure head fixed wedge block (10) is arranged in the groove. (6-1) and the lower end of the electrode pressure head (8) is wedged into the groove (6-1) through the matching inclined surface, and a clamping head insulating mica plate (11) is arranged on each matching inclined surface, and the clamping head insulating mica plate (11) is clamped between the electrode pressure head fixing wedge block (10) and the groove (6-1); the upper electrode pressure head (8) is arranged in the stepped hole of the electrode pressure head fixing wedge block (10), and a pressure head pressing plate (7) is arranged on the upper surface of the upper electrode pressure head (8), and a pressure head pressing plate (7) is arranged on the upper surface of the pressure head pressing plate (7). A plurality of pressure head fixing bolts (9) are arranged between the surface and the lower surface of the electrode pressure head fixing wedge block (10) to fix the upper electrode pressure head (8) in the stepped hole of the electrode pressure head fixing wedge block (10); a support block insulating mica board (5) is placed on the upper surface of the pressure head pressing plate (7), an adjustment support block (4) is arranged on the upper surface of the support block insulating mica board (5), and the adjustment support block (4) is tightly clamped between the upper surface of the groove (6-1) and the support block insulating mica board (5);

[0035] The arrangement and size of the lower fixed chuck (15) and its internal components are completely the same as those of the upper movable chuck (6). The lower fixed chuck (15) is arranged directly below the upper movable chuck (6). The groove opening of the lower fixed chuck (15) is vertically upward and corresponds to the position of the groove (6-1) of the upper movable chuck (6). The lower fixed chuck (15) and the upper movable chuck (6) are symmetrically arranged along the horizontal plane. The blank (13) is arranged between the upper electrode pressure head (8) and the lower electrode pressure head (14). ), the upper surface and the lower surface of the blank (13) are both flat and each is provided with a solder resist tantalum sheet (12); the lower fixed chuck (15) is fixed to the lower support plate (18) through a chuck pad (17), and the lower support plate (18) is located below the lower fixed chuck (15) and the chuck pad (17); two support columns (3) are symmetrically fixed between the lower support plate (18) and the upper support plate (2), and a plurality of moving wheels (16) are evenly arranged below the lower support plate (18);

[0036] The two poles of the pulsed DC power supply (19) are respectively connected to the upper electrode pressing head (8) and the lower electrode pressing head (14); the pulsed DC power supply (19), the upper electrode pressing head (8), two tantalum solder resist sheets (12), the blank (13) and the lower electrode pressing head (14) form a current closed loop; the blank (13) is connected to the thermocouple (20); and the force sensor (21) is connected to the hydraulic loading cylinder (1).

[0037] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the lower surface of the upper electrode press head (8) and the upper surface of the lower electrode press head (14) have a parallelism less than 0.02 and the roughness of the two surfaces is less than Ra0.8.

[0038] Such a design ensures that the upper electrode pressing head (8) and the lower electrode pressing head (14) can have good contact with the solder resist tantalum sheet (12) for electrical conduction. The rest is the same as the first specific implementation mode.

[0039] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the upper electrode pressure head (8) and the lower electrode pressure head (14) are made of heat-resistant and oxidation-resistant tungsten steel. The rest is the same as specific implementation method 1 or 2.

[0040] Specific implementation method 4: This implementation method is different from specific implementation methods 1 to 3 in that the insulating mica board (5) of the support block and the insulating mica board (11) of the clamp are both made of mica. The rest is the same as specific implementation methods 1 to 3.

[0041] Specific embodiment 5: This embodiment is different from the specific embodiment 4 in that the material of the upper movable chuck (6) and the lower fixed chuck (15) are both S136 die steel. The rest is the same as the specific embodiment 4.

[0042] Specific embodiment 6: This embodiment differs from specific embodiment 5 in that the surface area of ​​the solder resist tantalum sheet (12) is greater than or equal to the area of ​​the lower surface of the upper electrode pressure head (8), and the thickness of the solder resist tantalum sheet (12) is 0.05 mm to 0.1 mm. Other aspects are the same as specific embodiment 5.

[0043] Specific implementation method 7: This implementation method is different from specific implementation method 6 in that the thickness of the support block insulating mica board (5) and the clamp insulating mica board (11) are both 2 mm. The rest is the same as specific implementation method 6.

[0044] Specific embodiment eight: This embodiment is a method for using the pulse current rapid heating spheroidization device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet in specific embodiment one, and the specific process is as follows:

[0045] Step 1: cutting a blank (13) of a desired size from a high entropy alloy block sintered by powder metallurgy, wherein the blank (13) has two opposite end surfaces parallel to each other;

[0046] Step 2: grinding the surface oxide scale of the cut blank (13) to ensure good electrical conductivity;

[0047] Step 3: Welding a temperature monitoring thermocouple (20) onto the blank (13), placing a solder resist tantalum sheet (12) on the upper end surface of the lower electrode pressure head (14), and then placing the blank (13) connected with the thermocouple, and then placing another solder resist tantalum sheet (12) on the upper surface of the blank (13);

[0048] Step 4: The hydraulic loading cylinder (1) drives the upper movable chuck (6) and the upper electrode pressing head (8) to move downward together, so that the lower end surface of the upper electrode pressing head (8) contacts the solder resist tantalum sheet (12) on the upper surface of the blank (13), and applies a clamping load, the maximum load F does not exceed 5S, the unit is N, and the S is the area of ​​the lower surface of the upper electrode pressing head (8), the unit is mm 2 , to prevent the blank (13) from deforming at high temperatures;

[0049] Step 5: starting the pulsed DC power supply (19) to heat the blank (13) at a heating rate of 10°C / s to 30°C / s; using a thermocouple (20) to monitor the temperature of the blank (13) during the heating process;

[0050] Step 6: After the blank (13) is heated to a semi-solid temperature of 1175°C to 1225°C, isothermal holding is performed for 5s to 20s;

[0051] Step 7: Turn off the pulse DC power supply (19), and the hydraulic loading cylinder (1) drives the upper movable chuck (6) and the upper electrode pressing head (8) to move upward together;

[0052] Step 8: Use a clamp to remove the blank (13), and immediately transfer it to room temperature water for cooling to obtain a semi-solid blank.

[0053] Specific embodiment 9: This embodiment differs from specific embodiment 8 in that the voltage of the pulse DC power supply (19) in step 5 is 5V-10V, the current is 500A-1000A, and the power is 2.5kW-10kW. The rest is the same as specific embodiment 8.

[0054] Specific embodiment 10: This embodiment differs from specific embodiment 8 in that in step 7, the hydraulic loading cylinder (1) drives the upper movable clamp (6) and the upper electrode pressing head (8) to move upward by a distance of 50 mm to 100 mm. Other aspects are the same as specific embodiment 8.

[0055] The present invention is verified by the following tests:

[0056] Experiment 1: This experiment is a device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid heating and spheroidization by pulse current, such as Figure 1 and Figure 2 As shown, it specifically consists of a hydraulic loading cylinder (1), an upper support plate (2), a support column (3), an adjustment support block (4), a support block insulating mica plate (5), an upper movable chuck (6), a pressure head pressure plate (7), an upper electrode pressure head (8), a pressure head fixing bolt (9), an electrode pressure head fixing wedge (10), a chuck insulating mica plate (11), a solder resist tantalum sheet (12), a blank (13), a lower electrode pressure head (14), a lower fixed chuck (15), a moving wheel (16), a chuck pad (17), a lower support plate (18), a pulsed DC power supply (19), a thermocouple (20) and a force sensor (21);

[0057] The hydraulic loading cylinder (1) is fixed on the upper surface of the upper support plate (2), and the piston rod (1-1) of the hydraulic loading cylinder (1) passes through the upper support plate (2) and is slidably connected to the upper support plate (2), and the bottom surface of the piston rod (1-1) is fixedly connected to the upper surface of the upper movable chuck (6); the upper movable chuck (6) is arranged below the upper support plate (2), and a groove (6-1) is arranged between two opposite side walls of the movable chuck (6), and the two opposite inner walls in the groove (6-1) are inclined surfaces, and the opening of the groove (6-1) is vertically downward and the opening of the groove (6-1) gradually becomes smaller as it goes downward; the two opposite side walls in the electrode pressure head fixed wedge block (10) respectively match the two opposite inner walls in the groove (6-1), the upper surface of the electrode pressure head fixed wedge block (10) is a plane, and a stepped hole is arranged at the center of the electrode pressure head fixed wedge block (10), and the electrode pressure head fixed wedge block (10) is arranged in the groove. (6-1) and the lower end of the electrode pressure head (8) is wedged into the groove (6-1) through the matching inclined surface, and a clamping head insulating mica plate (11) is arranged on each matching inclined surface, and the clamping head insulating mica plate (11) is clamped between the electrode pressure head fixing wedge block (10) and the groove (6-1); the upper electrode pressure head (8) is arranged in the stepped hole of the electrode pressure head fixing wedge block (10), and a pressure head pressing plate (7) is arranged on the upper surface of the upper electrode pressure head (8), and a pressure head pressing plate (7) is arranged on the upper surface of the pressure head pressing plate (7). A plurality of pressure head fixing bolts (9) are arranged between the surface and the lower surface of the electrode pressure head fixing wedge block (10) to fix the upper electrode pressure head (8) in the stepped hole of the electrode pressure head fixing wedge block (10); a support block insulating mica board (5) is placed on the upper surface of the pressure head pressing plate (7), an adjustment support block (4) is arranged on the upper surface of the support block insulating mica board (5), and the adjustment support block (4) is tightly clamped between the upper surface of the groove (6-1) and the support block insulating mica board (5);

[0058] The arrangement and size of the lower fixed chuck (15) and its internal components are completely the same as those of the upper movable chuck (6). The lower fixed chuck (15) is arranged directly below the upper movable chuck (6). The groove opening of the lower fixed chuck (15) is vertically upward and corresponds to the position of the groove (6-1) of the upper movable chuck (6). The lower fixed chuck (15) and the upper movable chuck (6) are symmetrically arranged along the horizontal plane. The blank (13) is arranged between the upper electrode pressure head (8) and the lower electrode pressure head (14). ), the upper surface and the lower surface of the blank (13) are both flat and each is provided with a solder resist tantalum sheet (12); the lower fixed chuck (15) is fixed to the lower support plate (18) through a chuck pad (17), and the lower support plate (18) is located below the lower fixed chuck (15) and the chuck pad (17); two support columns (3) are symmetrically fixed between the lower support plate (18) and the upper support plate (2), and a plurality of moving wheels (16) are evenly arranged below the lower support plate (18);

[0059] The two poles of the pulsed DC power supply (19) are respectively connected to the upper electrode pressing head (8) and the lower electrode pressing head (14); the pulsed DC power supply (19), the upper electrode pressing head (8), two tantalum solder resist sheets (12), the blank (13) and the lower electrode pressing head (14) form a current closed loop; the blank (13) is connected to the thermocouple (20); and the force sensor (21) is connected to the hydraulic loading cylinder (1).

[0060] The lower surface of the upper electrode pressing head (8) and the upper surface of the lower electrode pressing head (14) have a parallelism less than 0.02 and the roughness of the two surfaces is less than Ra0.8; such a design ensures that the upper electrode pressing head (8) and the lower electrode pressing head (14) can have good contact with the solder resist tantalum sheet (12) for electrical conduction;

[0061] The upper electrode pressure head (8) and the lower electrode pressure head (14) are made of heat-resistant and oxidation-resistant tungsten steel;

[0062] The support block insulating mica board (5) and the clamp insulating mica board (11) are both made of mica;

[0063] The upper movable chuck (6) and the lower fixed chuck (15) are both made of S136 die steel;

[0064] The surface area of ​​the solder resist tantalum sheet (12) is equal to the area of ​​the lower surface of the upper electrode pressure head (8), and the thickness of the solder resist tantalum sheet (12) is 0.1 mm;

[0065] The area of ​​the lower surface of the upper electrode pressure head (8) is 1250 mm 2 ;

[0066] The thickness of the support block insulating mica board (5) and the clamp insulating mica board (11) are both 2 mm.

[0067] The method for using the above-mentioned pulse current rapid heating spheroidization device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet is as follows:

[0068] Step 1: Sintering high entropy alloy block Al from powder metallurgy 0.8 Co 0.5 Cr 1.5 Cutting a blank (13) of a desired size from CuFeNi, wherein the blank (13) has two opposite end faces parallel to each other;

[0069] Step 2: grinding the surface oxide scale of the cut blank (13) to ensure good electrical conductivity;

[0070] Step 3: Welding a temperature monitoring thermocouple (20) onto the blank (13), placing a solder resist tantalum sheet (12) on the upper end surface of the lower electrode pressure head (14), and then placing the blank (13) connected with the thermocouple, and then placing another solder resist tantalum sheet (12) on the upper surface of the blank (13);

[0071] Step 4: The hydraulic loading cylinder (1) drives the upper movable chuck (6) and the upper electrode pressing head (8) to move downward together, so that the lower end surface of the upper electrode pressing head (8) contacts the solder resist tantalum sheet (12) on the upper surface of the blank (13), and applies a clamping load, the load F being 6250N, to prevent the blank (13) from deforming at high temperature;

[0072] Step 5: starting the pulse DC power supply (19) to heat the blank (13) at a heating rate of 15°C / s; using a thermocouple (20) to monitor the temperature of the blank (13) during the heating process; the voltage of the pulse DC power supply (19) is 7.5V and the current is 800A;

[0073] Step 6: When the blank (13) is heated to a semi-solid temperature of 1225°C, the temperature is maintained isothermally for 10 seconds;

[0074] Step 7: Turn off the pulse DC power supply (19), and the hydraulic loading cylinder (1) drives the upper movable chuck (6) and the upper electrode pressing head (8) to move up 100 mm;

[0075] Step 8: Use clamps to remove the blank (13) and immediately transfer it to room temperature water for cooling to obtain Al 0.8 Co 0.5 Cr 1.5 CuFeNi semi-solid billet.

[0076] Figure 3 The Al sintered by powder metallurgy in step 1 of experiment 1 0.8 Co 0.5 Cr 1.5From the original microstructure diagram of the CuFeNi high entropy alloy billet, it can be seen that the grains are nearly equiaxed grains with an average grain size of 8.06±6.38μm.

[0077] Figure 4 Al obtained in step 8 of experiment 1 0.8 Co 0.5 Cr 1.5 The low magnification microstructure of the CuFeNi semi-solid billet taken by scanning electron microscope (SEM) shows that the average grain size of the semi-solid billet is 8.55±3.93μm, and the semi-solid grains are small. Figure 3 ), it can be seen that the grains are basically not coarsened. The shape factor of the solid phase grains reaches 0.83, which has a good spheroidization effect.

[0078] Figure 5 Al obtained in step 8 of experiment 1 0.8 Co 0.5 Cr 1.5 The microstructure image of the CuFeNi semi-solid billet taken under a scanning electron microscope (SEM) at a high magnification shows that a fine amplitude modulation decomposition structure is formed inside the solid phase grains, and a multi-scale multi-level structure is formed in the microstructure.

[0079] Figure 6 Al obtained in step 8 of experiment 1 0.8 Co 0.5 Cr 1.5 The microstructure of the CuFeNi semi-solid billet taken by transmission electron microscopy (TEM) shows that the stripe decomposition structure is a nanoscale structure. This fine structure is beneficial to the improvement of the mechanical properties of the semi-solid billet.

[0080] Figure 7 Al obtained in step 8 of experiment 1 0.8 Co 0.5 Cr 1.5 The oxidation weight gain of CuFeNi semi-solid billet under short-time heat preservation. The test results show that the oxidation degree of the billet is extremely low during the short-time heat preservation process. After heat preservation for 5s, 10s and 20s, the oxidation weight gain of the billet is only about 0.01mg / cm 2 , 0.02mg / cm 2 and 0.035mg / cm 2 It can be seen that the device and method of the present invention can significantly reduce the degree of oxidation in the preparation process of high entropy alloy semi-solid billet, improve the quality of the semi-solid billet, and do not require inert gas protection during preparation, thus saving costs.

Claims

1. A device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization, characterized in that The device for preparing a multi-level structure fine-grained high-entropy alloy semi-solid billet by pulse current rapid heating spheroidization comprises a hydraulic loading cylinder (1), an upper support plate (2), a support column (3), an adjustment support block (4), a support block insulating mica plate (5), an upper movable chuck (6), a pressure head pressure plate (7), an upper electrode pressure head (8), a pressure head fixing bolt (9), an electrode pressure head fixing wedge block (10), a chuck insulating mica plate (11), a solder resist tantalum sheet (12), a billet (13), a lower electrode pressure head (14), a lower fixed chuck (15), a moving wheel (16), a chuck pad (17), a lower support plate (18), a pulsed DC power supply (19), a thermocouple (20) and a force sensor (21); The hydraulic loading cylinder (1) is fixed on the upper surface of the upper support plate (2), and the piston rod (1-1) of the hydraulic loading cylinder (1) passes through the upper support plate (2) and is slidably connected to the upper support plate (2), and the bottom surface of the piston rod (1-1) is fixedly connected to the upper surface of the upper movable chuck (6); the upper movable chuck (6) is arranged below the upper support plate (2), and a groove (6-1) is arranged between two opposite side walls of the movable chuck (6), and two opposite inner walls of the groove (6-1) are inclined surfaces, and the opening of the groove (6-1) is vertically downward and the opening of the groove (6-1) gradually becomes smaller as it goes downward; the two opposite side walls of the electrode pressure head fixed wedge block (10) respectively match the two opposite inner walls of the groove (6-1), and the electrode pressure head fixed wedge block (10) is provided with a groove (6-1) between the two opposite side walls of the groove (6-1). The upper surface is a plane, a stepped hole is arranged at the center of the electrode pressure head fixing wedge block (10), the electrode pressure head fixing wedge block (10) is arranged in the groove (6-1) and the lower end of the electrode pressure head fixing wedge block (10) is wedged into the groove (6-1) through the matching inclined surfaces, and a clamping head insulating mica plate (11) is arranged on each matching inclined surface, and the clamping head insulating mica plate (11) is clamped between the electrode pressure head fixing wedge block (10) and the groove (6-1); the upper electrode pressure head (8) is arranged in the stepped hole of the electrode pressure head fixing wedge block (10), a pressure head pressing plate (7) is arranged on the upper surface of the upper electrode pressure head (8), and a plurality of pressure head fixing bolts (9) are arranged between the upper surface of the pressure head pressing plate (7) and the lower surface of the electrode pressure head fixing wedge block (10) to fix the upper electrode pressure head (8) in the stepped hole of the electrode pressure head fixing wedge block (10); A support block insulating mica plate (5) is placed on the upper surface of the pressure head pressing plate (7), an adjustment support block (4) is arranged on the upper surface of the support block insulating mica plate (5), and the adjustment support block (4) is tightly clamped between the upper surface of the groove (6-1) and the support block insulating mica plate (5); The arrangement and size of the lower fixed chuck (15) and its internal components are completely the same as those of the upper movable chuck (6). The lower fixed chuck (15) is arranged directly below the upper movable chuck (6). The groove opening of the lower fixed chuck (15) is vertically upward and corresponds to the position of the groove (6-1) of the upper movable chuck (6). The lower fixed chuck (15) and the upper movable chuck (6) are symmetrically arranged along the horizontal plane. The blank (13) is arranged between the upper electrode pressure head (8) and the lower electrode pressure head (14). ), the upper surface and the lower surface of the blank (13) are both flat and each is provided with a solder resist tantalum sheet (12); the lower fixed chuck (15) is fixed to the lower support plate (18) through a chuck pad (17), and the lower support plate (18) is located below the lower fixed chuck (15) and the chuck pad (17); two support columns (3) are symmetrically fixed between the lower support plate (18) and the upper support plate (2), and a plurality of moving wheels (16) are evenly arranged below the lower support plate (18); The two poles of the pulsed DC power supply (19) are respectively connected to the upper electrode pressing head (8) and the lower electrode pressing head (14); the pulsed DC power supply (19), the upper electrode pressing head (8), two tantalum solder resist sheets (12), the blank (13) and the lower electrode pressing head (14) form a current closed loop; the blank (13) is connected to the thermocouple (20); and the force sensor (21) is connected to the hydraulic loading cylinder (1).

2. The device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization according to claim 1 is characterized in that The lower surface of the upper electrode press head (8) and the upper surface of the lower electrode press head (14) have a parallelism less than 0.02 and the roughness of the two surfaces is less than Ra0.

8.

3. The device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization according to claim 1 is characterized in that The upper electrode pressing head (8) and the lower electrode pressing head (14) are made of temperature-resistant and oxidation-resistant tungsten steel.

4. The device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization according to claim 1 is characterized in that The support block insulating mica board (5) and the clamp insulating mica board (11) are both made of mica.

5. The device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization according to claim 1 is characterized in that The upper movable chuck (6) and the lower fixed chuck (15) are both made of S136 die steel.

6. The device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization according to claim 1 is characterized in that The surface area of ​​the solder resist tantalum sheet (12) is greater than or equal to the area of ​​the lower surface of the upper electrode pressure head (8), and the thickness of the solder resist tantalum sheet (12) is 0.05 mm to 0.1 mm.

7. The device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by pulse current rapid heating and spheroidization according to claim 1 is characterized in that The thickness of the support block insulating mica board (5) and the clamp insulating mica board (11) are both 2 mm.

8. The method for using the device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization as claimed in claim 1 is characterized in that The method for using the pulse current rapid heating spheroidization device to prepare a multi-level structure fine-grained high-entropy alloy semi-solid billet is as follows: Step 1: cutting a blank (13) of a desired size from a high entropy alloy block sintered by powder metallurgy, wherein the blank (13) has two opposite end surfaces parallel to each other; Step 2: grinding the surface oxide scale of the cut blank (13) to ensure good electrical conductivity; Step 3: Welding a temperature monitoring thermocouple (20) onto the blank (13), placing a solder resist tantalum sheet (12) on the upper end surface of the lower electrode pressure head (14), and then placing the blank (13) connected with the thermocouple, and then placing another solder resist tantalum sheet (12) on the upper surface of the blank (13); Step 4: The hydraulic loading cylinder (1) drives the upper movable chuck (6) and the upper electrode pressing head (8) to move downward together, so that the lower end surface of the upper electrode pressing head (8) contacts the solder resist tantalum sheet (12) on the upper surface of the blank (13), and applies a clamping load, the maximum load F does not exceed 5S, the unit is N, and the S is the area of ​​the lower surface of the upper electrode pressing head (8), the unit is mm 2 , to prevent the blank (13) from deforming at high temperatures; Step 5: starting the pulsed DC power supply (19) to heat the blank (13) at a heating rate of 10°C / s to 30°C / s; using a thermocouple (20) to monitor the temperature of the blank (13) during the heating process; Step 6: After the blank (13) is heated to a semi-solid temperature of 1175°C to 1225°C, the temperature is maintained isothermally for 5s to 20s; Step 7: Turn off the pulse DC power supply (19), and the hydraulic loading cylinder (1) drives the upper movable chuck (6) and the upper electrode pressing head (8) to move upward together; Step 8: Use a clamp to remove the blank (13), and immediately transfer it to room temperature water for cooling to obtain a semi-solid blank.

9. The method for using the device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by rapid pulse current heating and spheroidization according to claim 8 is characterized in that The pulse DC power supply (19) described in step 5 has a voltage of 5V to 10V, a current of 500A to 1000A, and a power of 2.5kW to 10kW.

10. The method for using the device for preparing multi-level structure fine-grained high-entropy alloy semi-solid billet by pulse current rapid heating and spheroidization according to claim 8 is characterized in that In step seven, the hydraulic loading cylinder (1) drives the upper movable clamp (6) and the upper electrode pressing head (8) to move upward together by a distance of 50 mm to 100 mm.