A lead-acid battery positive electrode and paste additive
By using modified 4BS, composite graphite fiber and liquid phase SiO2 as positive electrode and paste additives in lead-acid batteries, the problem of reduced mechanical strength of the positive plate during charge and discharge cycles is solved, significantly extending battery life and improving battery stability. sex.
Patent Information
- Application Number
- CN202211611764.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-15
AI Technical Summary
During the charge and discharge cycles of lead-acid batteries, the positive plate α-PbO2 is converted into β-PbO2 with low mechanical strength, which causes the conductive grid structure to weaken, the active material to fail and fall off, and shorten the battery life.
A lead-acid battery cathode and paste additive containing modified 4BS, composite graphite fiber and liquid SiO2 are used. Through the preparation method of modified 4BS and the preparation method of composite graphite fiber, a composite with relatively uniform particle size and high specific surface area is formed. material, enhances the mechanical strength and conductive properties of the positive plate, and extends battery life.
It significantly extends the cycle life of lead-acid batteries, prevents the positive plate active material from softening and falling off, and improves the initial capacity and stability of the battery.
Smart Images

Figure 693859DEST_PATH_IMAGE001
Abstract
Description
Technical Field
[0001] The invention relates to the field of lead-acid batteries and is a lead-acid battery positive electrode and paste additive. Background Art
[0002] In modern society, people have higher and higher requirements for the life of lead-acid batteries. The active materials of the positive plate of lead-acid batteries are composed of α-PbO2 and β-PbO2. The α-PbO2 structure is relatively coarse and has high mechanical strength, which is easy to connect. It can form a relatively coarse and strong skeleton and mesh structure, increase the mechanical strength of the plate, facilitate current conduction, stabilize the active material, etc. During the charge and discharge cycle of lead-acid batteries, the α-PbO2 of the positive plate will slowly transform into β-PbO2 with low mechanical strength, the conductive grid structure will be weakened, the active material will fail, soften, or even fall off, and thus the life of the lead-acid battery will end.
[0003] 4BS is added to the positive plate as a lead-acid battery positive electrode and paste additive to make 4BS type plates to produce lead-acid batteries. It mainly plays the role of crystal seeds. 4BS with suitable particle size can produce a large number of small and uniform particles when mixing with paste. It can prevent the plate from generating large particles of 4BS during high-temperature curing, thereby preventing the generation of large particles in the green plate and avoiding reducing the bonding force between the grid and the active substances in the lead paste. 4BS additives can shorten the curing time, increase the initial capacity of the battery, and extend the life. Summary of the invention
[0004] Purpose of the invention: To solve the above-mentioned problems, the present invention provides the following technical solutions.
[0005] The technical solution of the present invention is as follows:
[0006] The technical problem solved by the present invention is: to provide a positive electrode and paste additive for a lead-acid battery, which can inhibit the gradual conversion of α-PbO2 of the positive electrode plate into β-PbO2 with low mechanical strength during the charge and discharge cycle of the lead-acid battery, thereby avoiding the weakening of the conductive grid structure, the softening and even falling off of the active material, and the premature termination of the life of the lead-acid battery, thereby extending the service life of the lead-acid battery.
[0007] The technical solution adopted to solve the above technical problems is:
[0008] The invention provides a lead-acid battery positive electrode and paste additive comprising the following components in parts by weight: 6-10 parts of modified 4BS, 6-13 parts of composite graphite fibers and 5-12 parts of liquid SiO2.
[0009] According to the above scheme, the lead-acid battery positive electrode and paste additives contain the following components in parts by weight: 6-8 parts of modified 4BS, 7-11 parts of composite graphite fibers and 7-11 parts of liquid SiO2.
[0010] The preparation method of the composite graphite fiber of the invention comprises the following steps: adding graphite powder and polyphenylene sulfide in a mass ratio of 7-9:2-4 to a mixed solution of 1-3 volume times, heating the solution with microwave for 1-3 hours, injecting the solution into a 1-3 mol / L CTAB coagulation bath at a flow rate of 20-30 mL / h, performing shear flow, coagulation molding, traction orientation and roller rotation collection, drying with an infrared lamp to form composite graphene fibers, collecting with roller rotation, soaking with dilute nitric acid for 5-10 minutes, washing with an ethanol solution for 2-4 times, placing the fiber in a tubular furnace, introducing nitrogen, calcining at 700-800° C. and maintaining a constant temperature to obtain composite graphite fibers.
[0011] According to the above scheme, the mixed solution is anhydrous ethanol and hydrogen peroxide, and the mass ratio of anhydrous ethanol to hydrogen peroxide is 7-9:1-3.
[0012] According to the above scheme, the microwave heating frequency is 80-120KHZ, and the heating temperature is 40-50°C.
[0013] The preparation method of the modified 4BS of the present invention is as follows: Step 1: Add lead powder to water, and then add 5-8% of red lead and 8-10% of antimony trioxide in a mass ratio to mix; heat the reaction at a temperature of 280-350° C. in a reactor for 40-80 minutes, and cool the product to room temperature;
[0014] Step 2: Add 0.8-1.5 volume times of dilute sulfuric acid with a mass fraction of 40%-60% at a temperature of 40-60°C and continue to react for 70-90 minutes, then add 2%-4% anhydrous sodium sulfate with a mass fraction of lead powder and ultrasonically heat for 30-120 minutes, then filter, add the filter cake to a ball grinder for grinding after drying, and pass through a 100-180 mesh sieve to obtain modified 4BS.
[0015] According to the above scheme, it is characterized in that: the ultrasonic frequency is 60-100kHz and the ultrasonic temperature is 80-100°C.
[0016] Furthermore, according to the above scheme, the particle size of the modified 4BS is relatively evenly distributed in the range of 11-20 μm.
[0017] According to the above scheme, the liquid phase SiO2 adopts a silicon dioxide solution with a mass concentration of 17.5% to 33%, a specific surface area greater than 800m2 / g, and an average particle size less than 4 nanometers.
[0018] The preparation method of the lead-acid battery positive electrode and paste additive of the present invention is:
[0019] The composite graphene fiber is crushed, 4BS is added and mechanically premixed for 12-15 minutes, mixed evenly, and then heated and stirred for 60-90 minutes at a heating temperature of 80-120°C, and then SiO2 solution is added and stirred for 5-10 minutes to obtain a lead-acid battery positive electrode and paste additive.
[0020] The breakthrough of the present invention is that the charge and discharge cycle service life is improved without affecting the original performance of the lead-acid battery. DETAILED DESCRIPTION
[0021] The present invention is described below with reference to specific embodiments. It is hereby stated that the embodiments selected herein are only used to illustrate and explain the present invention and are not used to limit the present invention.
[0022] Example 1
[0023] This embodiment provides a lead-acid battery positive electrode and paste additive comprising the following components in parts by weight: 6-10 parts of modified 4BS, 6-13 parts of composite graphite fibers and 5-12 parts of liquid SiO2.
[0024] The lead-acid battery positive electrode and paste additives contain the following components by weight: 7 parts of modified 4BS, 8 parts of composite graphite fibers and 9 parts of liquid SiO2.
[0025] The preparation method of the composite graphite fiber of this embodiment is as follows: graphite powder and polyphenylene sulfide in a mass ratio of 8:3 are added to a mixed solution of 2 volume times and microwave heating is performed for 2 hours, the solution is then injected into a 2 mol / L CTAB coagulation bath in a coagulation bath at a flow rate of 25 mL / h, shear flow, coagulation molding, traction orientation and roller rotation collection are performed, and composite graphene fibers are formed by drying with an infrared lamp, collected by roller rotation, and then soaked in dilute nitric acid for 7 minutes, washed 3 times with ethanol solution, placed in a tubular furnace, and then nitrogen is introduced to calcine at 750°C and maintained at a constant temperature to obtain composite graphite fibers.
[0026] The mixed solution is anhydrous ethanol and hydrogen peroxide, and the mass ratio of anhydrous ethanol to hydrogen peroxide is 8:2.
[0027] The microwave heating frequency is 100KHZ and the heating temperature is 45°C.
[0028] The preparation method of the modified 4BS is:
[0029] Step 1: Add lead powder to water, and then add 7% red lead and 9% antimony trioxide in a mass ratio to mix; heat the reaction at a temperature of 310°C in a reactor for 60 minutes, and cool the product to room temperature;
[0030] Step 2: Add 1.2 volume times of 50% dilute sulfuric acid at a mass fraction and continue to react at a temperature of 50°C for 80 minutes, then add 3% anhydrous sodium sulfate as the mass of lead powder and ultrasonically heat for 80 minutes, then filter, dry the filter cake, add it to a ball grinder for grinding, and pass it through a 140-mesh sieve to obtain modified 4BS.
[0031] The ultrasonic frequency is 80kHz and the ultrasonic temperature is 90°C.
[0032] The particle size of the 4BS is evenly distributed within the range of 11 μm.
[0033] The liquid phase SiO2 adopts a silicon dioxide solution with a mass concentration of 17.5% to 33%, a specific surface area greater than 800m2 / g, and an average particle size less than 4 nanometers.
[0034] The preparation method of the lead-acid battery positive electrode and paste additive described in this embodiment is:
[0035] The composite graphene fiber is crushed, 4BS is added and mechanically premixed for 12-15 minutes, mixed evenly, and then heated and stirred for 60-90 minutes at a heating temperature of 80-120°C, and then SiO2 solution is added and stirred for 5-10 minutes to obtain a lead-acid battery positive electrode and paste additive.
[0036] Comparative Example 1
[0037] The difference between Comparative Example 1 and Example 1 is that the preparation method of the composite graphite fiber in Comparative Example 1 is different, and during the preparation process, an equal amount of distilled water is used instead of the mixed solution.
[0038] Comparative Example 2
[0039] The difference between Comparative Example 2 and Example 1 is that polyphenylene sulfide is not added during the preparation of the composite graphite fiber of Comparative Example 2.
[0040] Comparative Example 3
[0041] The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 uses an equal amount of graphite fibers instead of composite graphite fibers.
[0042] Comparative Example 4
[0043] The difference between Comparative Example 4 and Example 1 is that the preparation method of the modified 4BS in Comparative Example 4 is different, and the preparation method is:
[0044] Step 1: Add lead powder to water and mix with antimony trioxide in a mass ratio of 8-10%; heat the reaction at a temperature of 280-350°C in a reactor for 40-80 minutes, and cool the product to room temperature; then add anhydrous sodium sulfate in an amount of 2%-4% by mass of the lead powder and perform ultrasonic heating for 30-120 minutes, then filter, dry the filter cake, add it to a ball grinder for grinding, and pass it through a 100-180 mesh sieve to obtain modified 4BS.
[0045] Comparative Example 5
[0046] The difference between Comparative Example 5 and Example 1 is that what is added in Comparative Example 5 is common 4BS purchased on the market.
[0047] Comparative Example 6
[0048] The difference between Comparative Example 6 and Example 1 is that no modified 4BS is added in Comparative Example 6.
[0049] Comparative Example 7
[0050] The difference between Comparative Example 7 and Example 1 is that no composite graphite fiber is added in Comparative Example 6.
[0051] Comparative Example 8
[0052] The difference between Comparative Example 8 and Example 1 is that, in Comparative Example 6, a SIO2 solution having an average particle size of 10 nanometers is added.
[0053] Preparation of positive lead paste: 1000g of lead powder was weighed, and 100g, 200g and 300g of the positive electrode and paste additive prepared in Example 1 and 100g of the positive electrode and paste additive prepared in Comparative Examples 1-8 were added respectively, and stirred in a paste mixer for 30min, 100g of a dilute sulfuric acid solution with a density of 1.4g / cm3 and 100g of pure water were added and continued to stir evenly to obtain a uniform positive lead paste, and the above-mentioned lead paste was evenly applied to the positive electrode grid, and a positive electrode plate was obtained through rolling and curing processes, and the positive electrode plate was assembled with a negative electrode plate, a diaphragm and a sulfuric acid electrolyte to obtain a 12V7Ah lead-acid battery, and the battery was subjected to a life cycle test. The test results are shown in Table 1.
[0054] Table 1.
[0055]
[0056] As shown in Table 1, the positive electrode and paste additive prepared by the present invention are prepared by using modified 4BS, composite graphite fiber and liquid phase SIO2 in a certain ratio, which can significantly extend the cycle life of the battery; as shown in Comparative Examples 1-3, the composite graphite fiber added to the positive electrode and paste additive prepared by the present invention is better than ordinary graphite fiber and composite graphite fiber prepared by other methods, and the positive electrode and paste additive can significantly inhibit the positive electrode lead paste from crystallizing and softening the positive electrode lead paste, resulting in the shedding of the positive electrode active material, and the battery life is longer; as shown in Comparative Examples 4-5, the modified 4BS, composite graphite fiber and liquid phase SIO2 are prepared by using modified 4BS, composite graphite fiber and liquid phase SIO2 in a certain ratio, which can significantly extend the cycle life of the battery; as shown in Comparative Examples 4-5, the modified 4BS, composite graphite fiber and liquid phase SIO2 are prepared by using modified 4BS, composite graphite fiber and liquid phase SIO2 in a certain ratio, and the cycle life of the battery is significantly extended; as shown in Comparative Examples 5-6, the modified 4BS, composite graphite fiber and liquid phase SIO2 are prepared by using modified 4BS, composite graphite fiber and liquid phase SIO2 in a certain ratio, and the cycle life of the battery is significantly extended; as shown in Comparative Examples 6-7, the modified 4BS, composite graphite fiber and liquid phase SIO2 are prepared by using modified 4BS, composite graphite fiber and liquid phase SIO2 in a certain ratio, and the cycle life of the battery is significantly extended; as shown in Comparative Examples 7-8, the modified 4BS, composite graphite fiber and liquid phase SIO2 are prepared by using modified 4BS, composite graphite fiber and liquid phase SIO2 in a certain ratio, and the cycle life of the battery is significantly extended; as shown in Comparative Examples 8-9, the modified 4BS, composite graphite fiber and liquid phase SIO2 are prepared by using modified 4BS, composite graphite fiber and liquid phase SIO2 in a The preparation method of the modified 4BS and the use of ordinary 4BS are not as good as the 4BS prepared by the present invention in playing the role of crystal seeds, thereby extending the battery life; Comparative Examples 6-7 further illustrate that the positive electrode and paste additives added with the composite graphite fiber and modified 4BS prepared by the present invention can significantly improve the performance of the positive electrode lead paste, and are more stable during the operation of the battery; It can be seen from Comparative Example 8 that the positive electrode and paste additives prepared from nano-SIO2 solution with a small average particle size can more effectively inhibit the failure, softening and shedding of active materials in the battery during charge and discharge cycles, thereby extending the battery life.
[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A lead-acid battery positive electrode and paste additive, comprising the following components by weight: 6-10 parts of modified 4BS, 6-13 parts of composite graphite fiber and 5-12 parts of liquid SiO 2 ; The preparation method of the modified 4BS is: Step 1: Add lead powder to water, and then add 5-8% red lead and 8-10% antimony trioxide in a mass ratio to mix; heat the reaction at a temperature of 280-350°C in a reactor for 40-80 minutes, and cool the product to room temperature; Step 2: Add 0.8-1.5 volume times of dilute sulfuric acid with a mass fraction of 40%-60% at a temperature of 40-60°C and continue to react for 70-90 minutes, then add 2%-4% anhydrous sodium sulfate with a mass fraction of lead powder and perform ultrasonic heating for 30-120 minutes, then filter, dry the filter cake, add it to a ball grinder for grinding, and pass it through a 100-180 mesh sieve to obtain modified 4BS; the ultrasonic temperature is 80-100°C; The preparation method of the composite graphite fiber is as follows: adding graphite powder and polyphenylene sulfide with a mass ratio of 7-9:2-4 to a mixed solution with a volume multiple of 1-3, heating with microwave for 1-3h, injecting the solution into a 1-3mol / L CTAB coagulation bath at a flow rate of 20-30mL / h, performing shear flow, coagulation molding, traction orientation and roller rotation collection, drying with an infrared lamp to form a composite graphene fiber, collecting with roller rotation, soaking with dilute nitric acid for 5-10min, washing with ethanol solution for 2-4 times, placing in a tubular furnace, introducing nitrogen and calcining at 700-800°C and maintaining a constant temperature to obtain the composite graphite fiber; the mixed solution is anhydrous ethanol and hydrogen peroxide; the microwave heating temperature is 40-50°C; The liquid SiO 2 A silica solution with an average particle size of less than 4 nanometers is used.
2. The lead-acid battery positive electrode and paste additive according to claim 1, It is characterized in that The composition comprises the following components by weight: 6-8 parts of modified 4BS, 7-11 parts of composite graphite fiber and 7-11 parts of liquid SiO 2 .
3. The lead-acid battery positive electrode and paste additive according to claim 1, It is characterized in that The mass ratio of anhydrous ethanol to hydrogen peroxide is 7-9:1-3.
4. The lead-acid battery positive electrode and paste additive according to claim 1, It is characterized in that The microwave heating frequency is 80-120KHZ.
5. The lead-acid battery positive electrode and paste additive according to claim 1, Features: The ultrasonic frequency is 60-100kHz.
6. The lead-acid battery positive electrode and paste additive according to claim 1, It is characterized in that The particle size of the 4BS is evenly distributed in the range of 11-20 μm.
7. The lead-acid battery positive electrode and paste additive according to claim 1, Features: The liquid SiO 2 The mass concentration is 17.5% to 33% and the specific surface area is greater than 800m 2 / g.
8. The lead-acid battery positive electrode and paste additive according to claim 1, It is characterized in that The preparation method of the lead-acid battery positive electrode and paste additive is as follows: The composite graphene fiber was crushed, and 4BS was added for mechanical premixing for 12-15 minutes. The mixture was evenly mixed, and then heated and stirred for 60-90 minutes at a heating temperature of 80-120°C. SiO 2 The solution is stirred for 5-10 minutes to obtain a lead-acid battery positive electrode and a paste additive.