A fire-resistant and explosion-resistant ultra-high performance concrete and a preparation method thereof

By optimizing the formulation and maintenance process, refractory and explosion-resistant ultra-high performance concrete is prepared, which solves the problem of ultra-high performance concrete prone to explosion in fires, and achieves the improvement of fire resistance at high temperatures of 1050℃ and the satisfaction of building fire protection requirements.

CN115784682BActive Publication Date: 2024-11-29HUNAN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211403236.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-10
Publication Date
2024-11-29
Estimated Expiration
2042-11-10

AI Technical Summary

Technical Problem

Existing ultra-high performance concrete is prone to burst in fires, resulting in damage to building components. The existing fire resistance performance experimental temperature and dimensional effects are insufficient, which cannot meet the requirements of building fire protection specifications.

Method used

Utilizes optimized formulation of refractory and explosion-resistant ultra-high performance concrete, including cement, mineral blends, quartz sand, brown corundum, alumina powder, silicon carbide powder, steel slag, fiber materials and polymer water-absorbing resins, through specific mixing and curing The process is to form concrete with high fire resistance and explosion resistance.

Benefits of technology

The concrete does not burst after 2 hours of high temperature at 1050℃, and maintains a high residual strength, meets the requirements of building components of the first-level fire resistance grade, and is suitable for buildings, bridges, tunnels and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115784682B_ABST
    Figure CN115784682B_ABST
Patent Text Reader

Abstract

The present invention discloses a fire-resistant explosion-proof ultra-high performance concrete, comprising the following raw material components by weight: 1050-1600 parts of cement, 220-650 parts of mineral admixtures, 300-900 parts of quartz sand, 150-400 parts of quartz powder, 350-1200 parts of brown corundum, 0-500 parts of alumina powder, 0-450 parts of silicon carbide powder, 0-200 parts of steel slag, 15-50 parts of water reducer, 220-400 parts of fiber material, and 0-30 parts of polymer water-absorbing resin. The fire-resistant explosion-proof ultra-high performance concrete provided by the present invention not only does not burst after being subjected to a high temperature of 1050°C for 2 hours, but also still has a high residual strength after the disaster. The present invention also provides a preparation method of fire-resistant explosion-proof ultra-high performance concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete materials, and in particular to a fire-resistant and explosion-resistant ultra-high performance concrete and a preparation method thereof. Background Art

[0002] Ultra-high performance concrete (UHPC) is a new type of cement-based material in the construction field with ultra-high strength, ultra-high toughness and high durability. Due to its excellent mechanical properties and durability, UHPC has played an important role in the construction and reinforcement of super-high-rise buildings, large-span bridges, urban transportation, industrial plants and other engineering projects. However, in sudden disasters such as fires, due to the ultra-low water-cement ratio of UHPC, its interior is very dense. Under the action of high temperature, the moisture inside the UHPC cannot escape through the pores in time, resulting in excessive pore pressure, which eventually causes the UHPC to burst and fail. Compared with ordinary concrete components, UHPC components often have a larger "span" and a thinner protective layer. Once the concrete protective layer bursts and peels off in a fire, the steel bars are directly exposed to the fire temperature. The rapid deterioration of the steel bar performance will cause component damage and eventually lead to building collapse. Therefore, the study of the fire resistance of UHPC is of great significance. In order to prevent the "secondary disaster" of UHPC explosion causing damage to building components, we proposed a fire-resistant and explosion-resistant ultra-high performance concrete and its preparation method and application to improve the safety performance of UHPC structures in fires.

[0003] In the prior art, Chinese patent applications with publication numbers CN110563418A and CN104591635A disclose steam-free ultra-high strength concrete, but since the invention does not consider the fire resistance of ultra-high strength concrete, the invention is severely limited in its application in engineering fields such as construction engineering, underground engineering, and special industrial plants. Chinese patents with publication number CN 113563034 A disclose a kind of refractory ultra-high performance concrete cured at room temperature and its preparation method, the maximum experimental temperature of which is only 850°C, and the size effect has a significant impact on the high temperature performance of UHPC, and the cross-sectional size of its experimental test block is relatively small, so the test results are relatively unsafe. The fire resistance limit of beams and slabs with a fire resistance grade of one specified in the "GB 50016-2014 Code for Fire Protection Design of Buildings" should exceed two hours under the ISO standard heating system. The experimental temperature is still a certain distance from the high temperature of 1050°C corresponding to a heating time of 2 hours under the ISO standard heating system. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a fire-resistant and explosion-resistant ultra-high performance concrete. After being subjected to a high temperature of 1050°C for 2 hours, the fire-resistant and explosion-resistant ultra-high performance concrete not only does not burst, but also still has a high residual strength after the disaster. It fully meets the fire resistance limit requirements for beams, slabs and other building components with a first-level fire resistance grade in the existing "GB 50016-2014 Code for Fire Protection Design of Buildings", provides a practical solution for UHPC structural fire protection, and can be applied to buildings, bridges, tunnels, and even underground engineering and other fields.

[0005] In order to solve the above problems, the technical solution of the present invention is as follows:

[0006] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following raw material components by weight:

[0007] 1050-1600 parts of cement, 220-650 parts of mineral admixtures, 300-900 parts of quartz sand, 150-400 parts of quartz powder, 350-1200 parts of brown corundum, 0-500 parts of alumina powder, 0-450 parts of silicon carbide powder, 0-200 parts of steel slag, 15-50 parts of water reducing agent, 220-400 parts of fiber material, and 0-30 parts of polymer water-absorbing resin.

[0008] Furthermore, the cement includes at least one of silicate cement and calcium aluminate cement, wherein the silicate cement is PO42.5 grade or PO52.5 grade.

[0009] Furthermore, the mineral admixture includes silica fume and fly ash, wherein the SiO2 content of the silica fume is greater than 92% and the specific surface area is 18500m 2 / kg; fly ash density 2.55g / cm 3 , the loss on ignition is 3.86%.

[0010] Furthermore, the SiO2 content of the quartz sand is greater than 99%, and the particle size ranges from 20 to 40 meshes; the SiO2 content of the quartz powder is greater than 99%, and the particle size is 200 meshes.

[0011] Furthermore, the brown corundum has an Al2O3 content of more than 90% and a particle size of 0-5 mm; it is prepared by the following preparation method:

[0012] The three raw materials of high-alumina bauxite clinker, iron filings and anthracite are mixed and added into an electric arc furnace. After high-temperature calcination at 2250°C, after high-temperature melting and impurity reduction, they are cooled and crystallized to obtain brown fused blocks, which are then crushed to obtain brown corundum powder material.

[0013] Furthermore, the Al2O3 content in the alumina powder is greater than 99%, and the particle size ranges from 0.8 to 2.8 μm; the SiC content of the silicon carbide powder exceeds 99%, and the particle size ranges from 20 to 40 meshes; and the particle size of the steel slag is 0 to 5 mm.

[0014] Furthermore, the water reducing agent is a polycarboxylic acid powder water reducing agent with a water content of less than 2.8% and a water reduction rate of more than 25%.

[0015] Furthermore, the fiber material is at least one of steel fiber and synthetic fiber, wherein the steel fiber is copper-plated end hook steel fiber with a length of 13 mm, a diameter of 0.2 mm, and a tensile strength of 2000 MPa; the synthetic fiber is at least one of polypropylene fiber, polyvinyl alcohol fiber, nylon fiber, and polyoxymethylene fiber.

[0016] Furthermore, the average particle size of the polymer water-absorbing resin is 110-125 μm.

[0017] The present invention also provides a method for preparing fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following steps:

[0018] According to the raw material ratio of the fire-resistant and explosion-resistant ultra-high performance concrete, cement, mineral admixture, quartz sand, quartz powder, brown corundum, alumina powder, silicon carbide powder, and steel slag are poured into a mixer and mixed evenly, and then corresponding weight portions of water-reducing agent and polymer water-absorbing resin, as well as an appropriate amount of water are added, and stirring is continued, and then fiber materials are added and stirring is continued until the UHPC slurry is stirred in the mixer until it is completely fluidized, so as to obtain fire-resistant and explosion-resistant ultra-high performance concrete slurry;

[0019] The fire-resistant and explosion-resistant ultra-high performance concrete slurry is loaded into the mold, naturally cured at room temperature for 2 days before demolding, and steam cured for 48 hours. The temperature of the steam curing is controlled at above 90°C and the humidity is controlled at above 95%.

[0020] Compared with the prior art, the fire-resistant and explosion-resistant ultra-high performance concrete and the preparation method thereof provided by the present invention have the following beneficial effects:

[0021] The fire-resistant and explosion-resistant ultra-high performance concrete provided by the present invention improves the fire-resistant and explosion-resistant performance of concrete by optimizing the raw material formula of UHPC concrete. After being subjected to a high temperature of 1050°C for 2 hours, the ultra-high performance concrete not only does not burst, but also still has a high residual strength after the disaster, fully meeting the fire resistance limit requirements for beams, slabs and other building components with a first-class fire resistance grade in the existing "GB50016-2014 Building Design Fire Protection Code", providing a practical solution for UHPC structural fire protection, and can be applied to buildings, bridges, tunnels, and even underground engineering and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0023] Figure 1 This is the appearance of conventional UHPC after being heated to 400°C;

[0024] Figure 2 This is a comparison diagram of the appearance of the fire-resistant and explosion-resistant UHPC cubic compression test block before and after high temperature;

[0025] Figure 3 This is the residual compressive failure morphology diagram of the fire-resistant and explosion-resistant UHPC after high temperature of the present invention;

[0026] Figure 4 This is a comparison diagram of the appearance of the fire-resistant and explosion-resistant UHPC anti-bending test block of the present invention before and after high temperature;

[0027] Figure 5 This is a comparison diagram of the appearance of the fire-resistant and explosion-resistant UHPC dog-bone axis pulling test block of the present invention before and after high temperature. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to better understand the technical solutions in the embodiments of the present invention and to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are further described below in conjunction with the accompanying drawings.

[0029] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0030] The fire-resistant and explosion-resistant ultra-high performance concrete of the present invention comprises the following raw material components by weight:

[0031] 1050-1600 parts of cement, 220-650 parts of mineral admixtures, 300-900 parts of quartz sand, 150-400 parts of quartz powder, 350-1200 parts of brown corundum, 0-500 parts of alumina powder, 0-450 parts of silicon carbide powder, 0-200 parts of steel slag, 15-50 parts of water reducing agent, 220-400 parts of fiber material, and 0-30 parts of polymer water-absorbing resin.

[0032] Among them, the cement includes at least one of silicate cement and calcium aluminate cement, and the silicate cement is PO42.5 grade or PO52.5 grade; specifically, the cement content can be 1050 parts, 1100 parts, 1200 parts, 1300 parts, 1400 parts, 1500 parts or 1600 parts, or other values ​​within this range.

[0033] Mineral admixtures include silica fume and fly ash, among which the SiO2 content of silica fume is greater than 92% and the specific surface area is 18500m 2 / kg; fly ash density 2.55g / cm 3 , the loss on ignition is 3.86%; specifically, the content of the mineral admixture can be 220 parts, 300 parts, 400 parts, 500 parts, 600 parts or 650 parts, or other values ​​within this range.

[0034] The SiO2 content of quartz sand is greater than 99%, and the particle size range is 20-40 mesh; the SiO2 content of quartz powder is greater than 99%, and the particle size is 200 mesh; specifically, the content of quartz sand can be 300 parts, 350 parts, 400 parts, 450 parts, 500 parts, 550 parts, 600 parts, 650 parts, 700 parts, 750 parts, 800 parts, 850 parts or 900 parts, or other values ​​within this range; the content of quartz powder can be 150 parts, 200 parts, 250 parts, 300 parts, 350 parts or 400 parts, or other values ​​within this range.

[0035] The Al2O3 content of brown corundum is more than 90%, and its particle size is 0-5mm; it is prepared by the following preparation method:

[0036] The three raw materials of high-alumina bauxite clinker, iron filings and anthracite are mixed and added into an electric arc furnace. After high-temperature calcination at 2250°C, after high-temperature melting and impurity reduction, they are cooled and crystallized to obtain brown fused blocks, which are then crushed to obtain brown corundum powder material.

[0037] Specifically, the content of brown corundum can be 350 parts, 400 parts, 450 parts, 500 parts, 600 parts, 700 parts, 800 parts, 900 parts, 1000 parts, 1100 parts or 1200 parts, or other values ​​within this range.

[0038] The Al2O3 content in the alumina micropowder is greater than 99%, and the particle size range is 0.8-2.8μm; specifically, its content can be 0 parts, 50 parts, 100 parts, 120 parts, 150 parts, 170 parts, 200 parts, 230 parts, 250 parts, 300 parts, 350 parts, 400 parts or 500 parts, or other values ​​within this range.

[0039] The SiC content of the silicon carbide powder exceeds 99%, and the particle size range is 20-40 mesh; specifically, its content can be 0 parts, 50 parts, 60 parts, 70 parts, 80 parts, 100 parts, 120 parts, 150 parts, 200 parts, 250 parts, 300 parts, 350 parts, 400 parts or 450 parts, or other values ​​within this range.

[0040] The particle size of the steel slag is 0-5 mm. Specifically, its content can be 0 parts, 50 parts, 80 parts, 100 parts, 120 parts, 130 parts, 150 parts, 180 parts or 200 parts, or other values ​​within this range.

[0041] The water reducer is a polycarboxylic acid powder water reducer with a moisture content of less than 2.8% and a water reduction rate greater than 25%; specifically, its content can be 15 parts, 18 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts or 50 parts, or other values ​​within this range.

[0042] The fiber material is at least one of steel fiber and synthetic fiber, wherein the steel fiber is copper-plated end hook steel fiber with a length of 13 mm, a diameter of 0.2 mm and a tensile strength of 2000 MPa; the synthetic fiber is at least one of polypropylene fiber, polyvinyl alcohol fiber, nylon fiber and polyoxymethylene fiber; wherein the polypropylene fiber has a length of 12 mm, a diameter of 30 μm, an elastic modulus of 5 GPa and a melting point of about 165°C; the polyvinyl alcohol fiber has a length of 12 mm, a diameter of 20 μm, an elastic modulus of 16 GPa and a melting point of about 235°C; the nylon fiber has a length of 5 mm, a diameter of 20 μm, an elastic modulus of 8.4 GPa and a melting point of about 215°C; the polyoxymethylene fiber has a length of 12 mm, a diameter of 200 μm, an elastic modulus of 10 GPa and a melting point of about 165°C.

[0043] Specifically, the content of the fiber material may be 220 parts, 250 parts, 275 parts, 280 parts, 300 parts, 320 parts, 350 parts or 400 parts, or other values ​​within this range.

[0044] The average particle size of the polymer water-absorbing resin (SAP) is 110-125 μm, and its content can be 0 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts or 30 parts, or other values ​​within this range.

[0045] The method for preparing fire-resistant and explosion-resistant ultra-high performance concrete of the present invention comprises the following steps:

[0046] According to the above-mentioned raw material ratio of fire-resistant and explosion-resistant ultra-high performance concrete, cement, mineral admixture, quartz sand, quartz powder, brown corundum, alumina powder, silicon carbide powder, and steel slag are poured into a mixer and mixed evenly, and then corresponding weight portions of water-reducing agent and polymer water-absorbing resin, as well as an appropriate amount of water are added, and stirring is continued, and then fiber materials are added and stirring is continued until the UHPC slurry is stirred in the mixer until it is completely fluidized, so as to obtain fire-resistant and explosion-resistant ultra-high performance concrete slurry;

[0047] The fire-resistant and explosion-resistant ultra-high performance concrete slurry is loaded into the mold, naturally cured at room temperature for 2 days before demolding, and steam cured for 48 hours. The temperature of the steam curing is controlled at above 90°C and the humidity is controlled at above 95%.

[0048] The fire-resistant and explosion-resistant ultra-high performance concrete provided by the present invention is described in detail below through specific embodiments.

[0049] Example 1

[0050] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following components by weight:

[0051] 1284 parts of cement, 252 parts of silica fume, 118 parts of fly ash, 556 parts of brown corundum, 786 parts of quartz sand, 249 parts of quartz powder, 26 parts of water reducing agent, 255 parts of steel fiber, and 10 parts of polypropylene fiber.

[0052] The cement is PO42.5 grade silicate cement, with the measured compressive strength of 26.7MPa and 51.8MPa at 3 days and 28 days, and the measured flexural strength of 2.3MPa and 9.7MPa at 3 days and 28 days, respectively. The specific surface area is 342m 2 / kg.

[0053] The preparation method of the fire-resistant and explosion-resistant ultra-high performance concrete of this embodiment is as follows:

[0054] Pour cement, brown corundum, quartz sand, quartz powder, silica fume and fly ash into a mixer and mix evenly for 3 minutes, then add corresponding weight portions of water and water, continue to stir evenly for 10 minutes, then add steel fiber and continue to stir evenly for 3 minutes, finally add synthetic fiber and stir for 3 minutes, until the UHPC slurry is stirred in the mixer until it is completely fluidized, and obtain fire-resistant and explosion-resistant ultra-high performance concrete slurry;

[0055] The UHPC slurry was loaded into the mold, and then placed on a small vibration table for 30 seconds to reduce the internal porosity of the test block. A large amount of heat was released during the hydration process of UHPC, so water was sprinkled on the surface of the UHPC to keep the surface of the UHPC moist, and then covered with a film, and the mold was removed after natural curing at room temperature for 2 days. The demolded UHPC test block was steam cured for 48 hours, and the temperature and humidity of the steam curing were controlled at 90 and 95% respectively.

[0056] UHPC was prepared according to the above method. The prepared UHPC was heated to 1050°C in a muffle furnace. After being kept at a high temperature of 1050°C for 2 hours, the heating program ended automatically. After the furnace was naturally cooled to room temperature, the test block was taken out.

[0057] The UHPC in Example 1 after high temperature was subjected to residual compressive strength test, UHPC prism flexural strength test after high temperature, and UHPC dog bone axial tensile strength test after high temperature. The test results are shown in Table 1:

[0058] Table 1: UHPC performance test results after high temperature in Example 1

[0059]

[0060] It should be noted that the test method for the compressive strength of UHPC cubes after high temperature in the present invention is as follows:

[0061] 1. Check the size and shape of the UHPC cube test block;

[0062] 2. Wipe clean the surface of the UHPC cube test block and the upper and lower pressure plates;

[0063] 3. The side of the specimen when it is formed is the pressure-bearing surface. The specimen should be placed on the lower pressure plate or pad of the testing machine, and the center of the specimen should be aligned with the center of the lower pressure plate of the testing machine;

[0064] 4. Start the testing machine, and the surface of the test piece should be in uniform contact with the upper and lower pressure plates or steel pads;

[0065] 5. Loading should be applied continuously and evenly during the test. Preloading should be performed to ensure that the upper pressure plate is completely in contact with the pressure surface of the test block. Since the residual strength of UHPC decreases significantly after high temperature, in order to ensure that preloading does not cause initial damage to UHPC, preloading is performed at a rate of 5mm / min to 2kN, and the load is held for 20 seconds after reaching the target force value of 2kN;

[0066] 6. After the pre-loading stage, the formal loading stage begins. The loading speed is controlled according to the stress and is 1.0MPa / s.

[0067] After UHPC hardens, there are still a lot of unhydrated particles such as cement and active admixtures inside. After high temperatures of 200℃ and 400℃, the high temperature promotes the further hydration of cement and active admixtures inside UHPC. Therefore, the compressive strength after high temperatures of 200℃ and 400℃ is significantly improved compared with the compressive strength at room temperature. After a series of experimental tests and literature data statistics, the target force value in the formal loading stage should be greater than 1.3 times the compressive strength of the UHPC specimen at room temperature, but note that the specimen failure load cannot be greater than the full range of the press, and should be less than 80% of the full range of the press.

[0068] Taking the UHPC of Example 1 as an example, the change of the compressive strength of UHPC after high temperature with temperature is shown in Table 2. The compressive strength of each temperature group is the average compressive strength of the three test blocks.

[0069] Table 2: Changes of UHPC compressive strength after high temperature with temperature

[0070]

[0071] The method for the flexural strength test of the UHPC prism after high temperature of the present invention is as follows:

[0072] 1. Check the size and shape of the UHPC prism.

[0073] 2. Before placing the specimen in the test device, the surface of the specimen should be wiped clean and the loading line position should be drawn on the side of the specimen.

[0074] 3. The pressure-bearing surface of the specimen should be the side surface of the specimen when it is formed. The contact surface between the support and the pressure-bearing surface and the cylinder should be stable and uniform, otherwise it should be leveled.

[0075] 4. To ensure that preloading does not cause initial damage to UHPC, preload at a rate of 5 mm / min to 2 kN, and hold the load for 20 seconds after reaching the target force value of 2 kN.

[0076] 5. After the pre-loading stage, the formal loading stage begins. During the test, the load should be applied continuously and evenly, and the loading speed should be 0.05MPa / s.

[0077] The method for the UHPC dog bone high temperature rear axial tensile strength test of the present invention is as follows:

[0078] 1. Since the UHPC test block has experienced high temperature damage after high temperature, the internal defects are more significant. In order to ensure that the UHPC dog bone test block is completely axially tensile, the UHPC dog bone test block should be destroyed in the straight line segment and carbon fiber cloth should be pasted on the surface of the test block. Apply carbon fiber impregnation glue at the variable section, paste carbon fiber cloth, and then apply carbon fiber impregnation glue on the carbon fiber cloth again. To avoid the test block from being damaged at the variable section, the length of the carbon fiber cloth should be greater than the length of the arc segment of the variable section.

[0079] 2. In order to observe the development of cracks in the straight section of the test block, paint the straight section with white paint.

[0080] 3. The cross-sectional size of the UHPC dog bone test block is 50×50cm 2 . In the preloading stage, force loading is first performed, first loaded to 2kN, and then the load is unloaded to zero. The force and displacement values ​​are reset to zero, and the formal loading stage begins. Because UHPC has been subjected to high temperatures, its brittle characteristics are more obvious when it is damaged by tension. In order to obtain a complete stress-strain curve and reduce cracks caused by excessive loading rates, the formal loading is carried out according to displacement control, and the loading is continued at 0.05mm / min until the dog-bone specimen reaches the maximum bearing capacity. In the strain softening stage, the loading rate is increased to 0.5mm / min. When the controlled load drops to 40% of the maximum load, the test is stopped.

[0081] Please refer to Figures 1 to 5 ,in Figure 1 This is the appearance of conventional UHPC after being heated to 400°C; Figure 2 This is a comparison of the appearance of the fire-resistant and explosion-resistant UHPC before and after high temperature. Figure 2 (a) shows the appearance of UHPC at room temperature. Figure 2 (b) shows the appearance of UHPC after 1050℃; Figure 3 This is the residual compressive failure morphology diagram of the fire-resistant and explosion-resistant UHPC after high temperature of the present invention, where Figure 3 (a) is a schematic diagram showing the test process. Figure 3 (b) Schematic diagram showing test results; Figure 4 This is a comparison of the appearance of the fire-resistant and explosion-resistant UHPC anti-bending test block of the present invention before and after high temperature. Figure 4 (a) shows the appearance of the flexural test piece before high temperature. Figure 4 (b) represents the appearance of the flexural test piece after high temperature; Figure 5 This is a comparison of the appearance of the fire-resistant and explosion-resistant UHPC dog bone axis pulling test block before and after high temperature. Figure 5 (a) shows the appearance of the test piece before high temperature. Figure 5 (b) shows the appearance of the test piece after high temperature. Figure 1 It can be seen that conventional UHPC suffered severe explosion after high temperature of 400℃; Figure 2 , Figure 4 , Figure 5 It can be seen that after being subjected to a high temperature of 1050°C, the UHPC of the present invention did not explode; Figure 3 It can be seen that UHPC still has a high residual strength after being heated to 1050℃.

[0082] It should be noted that the high temperature test of the present invention is to keep the temperature constant at 1050°C for 2 hours. The internal temperature of the concrete is very close to the external temperature. At this time, it is reliable to use the external temperature to characterize the internal temperature of the concrete and to establish the relationship between the mechanical properties of the concrete and the temperature. If the constant temperature process is not set, the internal temperature of the concrete will be significantly different from its external temperature, and there will be a large deviation when the external temperature is used directly to replace the internal temperature of the concrete. In the post-disaster assessment of building fires, it is necessary to determine the relationship between the mechanical properties of UHPC and its internal experienced temperature. Only on this basis can the residual bearing capacity of building components after fire be evaluated.

[0083] Example 2

[0084] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following components by weight:

[0085] 1298 parts of cement, 285 parts of silica fume, 163 parts of fly ash, 575 parts of brown corundum, 773 parts of quartz sand, 242 parts of quartz powder, 25 parts of water reducing agent, 257 parts of steel fiber, 8 parts of polypropylene fiber, and 5 parts of polyvinyl alcohol fiber.

[0086] The preparation and curing process of the fire-resistant and explosion-resistant ultra-high performance concrete of this embodiment refer to that of Embodiment 1.

[0087] The UHPC prepared in Example 2 was heated to 1050° C. in a muffle furnace. After being kept at 1050° C. for 2 hours, the heating program automatically ended. After the furnace was naturally cooled to room temperature, the test piece was taken out.

[0088] The UHPC of Example 2 after high temperature was subjected to residual compressive strength test, UHPC prism flexural strength test after high temperature, and UHPC dog bone axial tensile strength test after high temperature. The test results are shown in Table 3:

[0089] Table 3: Example 2 UHPC performance test results after high temperature

[0090]

[0091]

[0092] Example 3

[0093] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following components by weight:

[0094] 1321 parts of cement, 256 parts of silica fume, 132 parts of fly ash, 763 parts of brown corundum, 569 parts of quartz sand, 251 parts of quartz powder, 33 parts of water reducing agent, 264 parts of steel fiber, 10 parts of polypropylene fiber, and 5 parts of nylon fiber.

[0095] The preparation and curing process of the fire-resistant and explosion-resistant ultra-high performance concrete of this embodiment refer to that of Embodiment 1.

[0096] The UHPC prepared in Example 3 was heated to 1050° C. in a muffle furnace. After being kept at 1050° C. for 2 hours, the heating program automatically ended. After the furnace naturally cooled to room temperature, the test piece was taken out.

[0097] The UHPC of Example 3 after high temperature was subjected to residual compressive strength test, UHPC prism flexural strength test after high temperature, and UHPC dog bone axial tensile strength test after high temperature. The test results are shown in Table 4:

[0098] Table 4: UHPC performance test results after high temperature in Example 3

[0099]

[0100] Example 4

[0101] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following components by weight:

[0102] 1263 parts of cement, 238 parts of silica fume, 152 parts of fly ash, 653 parts of brown corundum, 669 parts of quartz sand, 232 parts of quartz powder, 36 parts of water reducing agent, 263 parts of steel fiber, 12 parts of polypropylene fiber, and 3 parts of polyvinyl alcohol fiber.

[0103] The preparation and curing process of the fire-resistant and explosion-resistant ultra-high performance concrete of this embodiment refer to that of Embodiment 1.

[0104] The UHPC prepared in Example 4 was heated to 1050° C. in a muffle furnace. After being kept at a high temperature of 1050° C. for 2 hours, the heating program automatically ended. After the furnace was naturally cooled to room temperature, the test piece was taken out.

[0105] The UHPC of Example 4 after high temperature was subjected to residual compressive strength test, UHPC prism flexural strength test after high temperature, and UHPC dog bone axial tensile strength test after high temperature. The test results are shown in Table 5:

[0106] Table 5: UHPC performance test results after high temperature in Example 4

[0107]

[0108] Example 5

[0109] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following components by weight:

[0110] 1361 parts of cement, 252 parts of silica fume, 143 parts of fly ash, 718 parts of brown corundum, 136 parts of steel slag, 436 parts of quartz sand, 247 parts of quartz powder, 25 parts of water reducing agent, 262 parts of steel fiber, 13 parts of polyoxymethylene fiber, and 13 parts of SAP.

[0111] The preparation and curing process of the fire-resistant and explosion-resistant ultra-high performance concrete of this embodiment refer to that of Embodiment 1.

[0112] The UHPC prepared in Example 5 was heated to 1050° C. in a muffle furnace. After being kept at 1050° C. for 2 hours, the heating program automatically ended. After the furnace was naturally cooled to room temperature, the test piece was taken out.

[0113] The UHPC in Example 5 after high temperature was subjected to residual compressive strength test, UHPC prism flexural strength test after high temperature, and UHPC dog bone axial tensile strength test after high temperature. The test results are shown in Table 6:

[0114] Table 6: UHPC performance test results after high temperature in Example 5

[0115]

[0116] Example 6

[0117] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following components by weight:

[0118] 1255 parts of cement, 213 parts of silica fume, 147 parts of fly ash, 572 parts of brown corundum, 764 parts of quartz sand, 262 parts of alumina powder, 182 parts of quartz powder, 31 parts of water reducing agent, 253 parts of steel fiber, and 14 parts of polyoxymethylene fiber.

[0119] The preparation and curing process of the fire-resistant and explosion-resistant ultra-high performance concrete of this embodiment refer to that of Embodiment 1.

[0120] The UHPC prepared in Example 6 was heated to 1050° C. in a muffle furnace. After being kept at 1050° C. for 2 hours, the heating program automatically ended. After the furnace naturally cooled to room temperature, the test piece was taken out.

[0121] The UHPC of Example 6 after high temperature was subjected to residual compressive strength test, UHPC prism flexural strength test after high temperature, and UHPC dog bone axial tensile strength test after high temperature. The test results are shown in Table 7:

[0122] Table 7: UHPC performance test results after high temperature in Example 6

[0123]

[0124]

[0125] Example 7

[0126] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following components by weight:

[0127] 1316 parts of cement, 214 parts of silica fume, 142 parts of fly ash, 560 parts of brown corundum, 742 parts of quartz sand, 268 parts of silicon carbide powder, 173 parts of quartz powder, 29 parts of water reducing agent, 252 parts of steel fiber, 10 parts of polypropylene fiber, and 11 parts of SAP.

[0128] The preparation and curing process of the fire-resistant and explosion-resistant ultra-high performance concrete of this embodiment refer to that of Embodiment 1.

[0129] The UHPC prepared in Example 7 was heated to 1050° C. in a muffle furnace. After being kept at a high temperature of 1050° C. for 2 hours, the heating program automatically ended. After the furnace was naturally cooled to room temperature, the test piece was taken out.

[0130] The UHPC of Example 7 after high temperature was subjected to residual compressive strength test, UHPC prism flexural strength test after high temperature, and UHPC dog bone axial tensile strength test after high temperature. The test results are shown in Table 8:

[0131] Table 8: UHPC performance test results after high temperature in Example 7

[0132]

[0133] Example 8

[0134] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following components by weight:

[0135] 321 parts of calcium aluminate cement, 1056 parts of Portland cement, 273 parts of silica fume, 172 parts of fly ash, 1097 parts of brown corundum, 152 parts of steel slag, 324 parts of quartz sand, 164 parts of alumina powder, 67 parts of silicon carbide powder, 158 parts of quartz powder, 28 parts of water reducing agent, 261 parts of steel fiber, 5 parts of polypropylene fiber, 15 parts of polyoxymethylene fiber, and 8 parts of SAP.

[0136] The preparation and curing process of the fire-resistant and explosion-resistant ultra-high performance concrete of this embodiment refer to that of Embodiment 1.

[0137] The UHPC prepared in Example 8 was heated to 1050° C. in a muffle furnace. After being kept at a high temperature of 1050° C. for 2 hours, the heating program automatically ended. After the furnace was naturally cooled to room temperature, the test piece was taken out.

[0138] The UHPC of Example 8 after high temperature was subjected to residual compressive strength test, UHPC prism flexural strength test after high temperature, and UHPC dog bone axial tensile strength test after high temperature. The test results are shown in Table 9:

[0139] Table 9: UHPC performance test results after high temperature in Example 8

[0140]

[0141] Example 9

[0142] A fire-resistant and explosion-resistant ultra-high performance concrete, comprising the following components by weight:

[0143] 1254 parts of cement, 223 parts of silica fume, 189 parts of fly ash, 652 parts of brown corundum, 126 parts of quartz sand, 468 parts of alumina powder, 423 parts of silicon carbide powder, 186 parts of quartz powder, 38 parts of water reducing agent, 256 parts of steel fiber, and 27 parts of polypropylene fiber.

[0144] The preparation and curing process of the fire-resistant and explosion-resistant ultra-high performance concrete of this embodiment refer to that of Embodiment 1.

[0145] The UHPC prepared in Example 7 was heated to 1050° C. in a muffle furnace. After being kept at a high temperature of 1050° C. for 2 hours, the heating program automatically ended. After the furnace was naturally cooled to room temperature, the test piece was taken out.

[0146] The UHPC of Example 7 after high temperature was subjected to residual compressive strength test, UHPC prism flexural strength test after high temperature, and UHPC dog bone axial tensile strength test after high temperature. The test results are shown in Table 10:

[0147] Table 10: UHPC performance test results after high temperature in Example 9

[0148]

[0149]

[0150] It can be seen from the above embodiments that the fire-resistant and explosion-resistant ultra-high performance concrete of the present invention has strong fire-resistant and explosion-resistant performance, and its principle is as follows:

[0151] Since quartz sand undergoes a high-temperature phase transition at around 573°C, during the transition from α phase to β phase, the quartz sand expands in volume, cracks occur in the interface transition zone (ITZ zone) between aggregate and cement, and cracks also appear in the quartz sand aggregate. As the temperature further increases, damage accumulates in the interface transition zone, eventually leading to local cracking and damage, increasing the risk of UHPC bursting. The raw material for the preparation of brown corundum, bauxite, has undergone secondary high-temperature calcination, and has a small linear change rate and volume change rate after high temperature. It can still maintain a good interface transition zone with cement stone after experiencing high temperature. Therefore, compared with the high-temperature performance of quartz sand, corundum has better thermal stability, and adding it to UHPC can significantly improve the mechanical properties of UHPC after high temperature.

[0152] In conventional UHPC, C3S, C2S and water in cement clinker react to form CSH, which is the main source of concrete strength. Quartz sand plays the role of a skeleton. Compared with quartz sand, the main mineral in corundum is α-Al2O3, and its crystal structure is the closest hexagonal packing of oxygen ions, the distance between particles is small, and the anionic and cationic bonds transition from ionic bonds to covalent bonds. Its covalent bond characteristics make it have a higher hardness. The hardness of corundum is 9, which is higher than the hardness of quartz sand by 6. Therefore, the skeleton effect of corundum is more significant. Ca(OH)2 produced during cement hydration is dehydrated at high temperature to form a decomposition product CaO. CaO undergoes the following chemical reaction with Al2O3 in corundum under high temperature:

[0153] CaO+α-Al2O3→CA

[0154] CA+α-Al2O3→CA2

[0155] CA and CA2 crystals can form a denser structure at high temperatures, which is why the test block can still maintain a certain strength after being calcined at 1050°C.

[0156] Alumina powder has a significant effect on promoting cement hydration. Alumina powder provides nucleation sites for the precipitation of hydration products, promoting cement hydration. The smaller the particle size, the more nucleation sites it provides for hydration products. After high temperature of 1000℃, alumina powder further densifies the matrix, and the formation of CA2 makes the powder particles in the matrix combine with each other, and the binding force is improved. Therefore, alumina powder can significantly improve the mechanical properties of UHPC after high temperature.

[0157] Silicon carbide has a higher thermal conductivity than quartz sand, and can reduce the cross-sectional thermal stress gradient and thermal stress to a certain extent in UHPC. In addition, silicon carbide has high hardness, a melting point of up to 2700°C, and stable chemical properties. Compared with quartz sand, which undergoes a high-temperature phase transition at around 573°C, silicon carbide has better thermal stability and can better fill the gaps between aggregates, making the skeleton structure more stable.

[0158] Compared with the prior art, the fire-resistant and explosion-resistant ultra-high performance concrete and the preparation method thereof provided by the present invention have the following beneficial effects:

[0159] The fire-resistant and explosion-resistant ultra-high performance concrete provided by the present invention improves the fire-resistant and explosion-resistant performance of concrete by optimizing the raw material formula of UHPC concrete. After being subjected to a high temperature of 1050°C for 2 hours, the ultra-high performance concrete not only does not burst, but also still has a high residual strength after the disaster, fully meeting the fire resistance limit requirements for beams, slabs and other building components with a first-class fire resistance grade in the existing "GB50016-2014 Building Design Fire Protection Code", providing a practical solution for UHPC structural fire protection, and can be applied to buildings, bridges, tunnels, and even underground engineering and other fields.

[0160] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations made to these embodiments without departing from the principles and spirit of the present invention are still within the scope of protection of the present invention.

Claims

1. A fire-resistant and explosion-resistant ultra-high performance concrete, characterized in that: The composition includes the following raw materials by weight: 1050-1600 parts of cement, 220-650 parts of mineral admixtures, 300-900 parts of quartz sand, 150-400 parts of quartz powder, 350-1200 parts of brown corundum, 164-500 parts of alumina powder, 67-450 parts of silicon carbide powder, 152-200 parts of steel slag, 15-50 parts of water reducing agent, 220-400 parts of fiber material, 8-30 parts of polymer water-absorbing resin; The brown corundum has an Al2O3 content of more than 90% and a particle size of 0-5 mm; it is prepared by the following preparation method: The three raw materials of high-alumina bauxite clinker, iron scraps and anthracite are mixed and added into an electric arc furnace, calcined at 2250℃, melted at high temperature and reduced with impurities, cooled and crystallized to obtain brown frit, which is then crushed to obtain brown corundum powder material; The Al2O3 content of the alumina powder is greater than 99%, and the particle size range is 0.8-2.8μm; the SiC content of the silicon carbide powder exceeds 99%, and the particle size range is 20-40 mesh; The fiber material includes steel fiber and synthetic fiber, wherein the steel fiber is copper-plated end hook steel fiber with a length of 13 mm, a diameter of 0.2 mm, and a tensile strength of 2000 MPa; the synthetic fiber is at least one of polypropylene fiber, polyvinyl alcohol fiber, nylon fiber, and polyoxymethylene fiber.

2. The fire-resistant and explosion-resistant ultra-high performance concrete according to claim 1, characterized in that: The cement comprises at least one of silicate cement and calcium aluminate cement, wherein the silicate cement is of PO42.5 grade or PO52.5 grade.

3. The fire-resistant and explosion-resistant ultra-high performance concrete according to claim 1, characterized in that: Mineral admixtures include silica fume and fly ash. The SiO2 content of silica fume is greater than 92% and the specific surface area is 18500m 2 / kg; fly ash density 2.55g / cm 3 , the loss on ignition is 3.86%.

4. The fire-resistant and explosion-resistant ultra-high performance concrete according to claim 1, characterized in that: The SiO2 content of the quartz sand is greater than 99%, and the particle size ranges from 20 to 40 meshes; the SiO2 content of the quartz powder is greater than 99%, and the particle size is 200 meshes.

5. The fire-resistant and explosion-resistant ultra-high performance concrete according to claim 1, characterized in that: The particle size of the steel slag is 0-5 mm.

6. The fire-resistant and explosion-resistant ultra-high performance concrete according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid powder water reducing agent with a water content of less than 2.8% and a water reduction rate of more than 25%.

7. The fire-resistant and explosion-resistant ultra-high performance concrete according to claim 1, characterized in that: The average particle size of the polymer water-absorbing resin is 110-125 μm.

8. A method for preparing fire-resistant and explosion-resistant ultra-high performance concrete, characterized in that: The steps include: According to the raw material ratio of the fire-resistant and explosion-resistant ultra-high performance concrete of claim 1, cement, mineral admixture, quartz sand, quartz powder, brown corundum, alumina powder, silicon carbide powder, and steel slag are poured into a mixer and mixed evenly, and then corresponding weight portions of water-reducing agent and polymer water-absorbing resin, as well as an appropriate amount of water are added, and stirring is continued, and then fiber materials are added and stirring is continued until the UHPC slurry is stirred in the mixer until it is completely fluidized, so as to obtain fire-resistant and explosion-resistant ultra-high performance concrete slurry; The fire-resistant and explosion-resistant ultra-high performance concrete slurry is loaded into the mold, naturally cured at room temperature for 2 days before demolding, and steam cured for 48 hours. The temperature of the steam curing is controlled at above 90°C and the humidity is controlled at above 95%.

Citation Information

Patent Citations

  • Anti-cracking steam-curing-free ultra-high-strength high-toughness concrete and preparation method thereof

    CN104591635A

  • Steam-curing-free ultra-high performance concrete and preparation method thereof

    CN110563418A

  • Normal-temperature curing fire-resistant ultra-high-performance concrete and preparation method thereof

    CN113563034A

  • Wear-resistant and antiknock concrete and preparation method thereof

    CN105801039A

  • Strong explosion-proof high-fire-resistance UHPC as well as preparation method and application thereof