A LiB electrode material and its preparation method and application

By attaching an anti-overflow layer of nanomaterial or skeleton material to the surface of LiB alloy, the overflow problem of LiB alloy electrode materials in high temperature and complex mechanical environments is solved, and the thermal stability and environmental adaptability of thermal batteries are improved.

CN115799442BActive Publication Date: 2024-11-26INST OF ELECTRONICS ENG CHINA ACAD OF ENG PHYSICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211520092.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-11-26
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

LiB alloys are prone to metal lithium overflow as thermal battery electrode material, resulting in the problem of thermal runaway from the battery, especially in high temperature and complex mechanical environments.

Method used

The anti-overflow layer is prepared by a mixture of nanomaterials or framework materials, which is attached to the surface of LiB alloy, and the overflow of liquid metal lithium is inhibited by adhesion and sealing. The anti-overflow layer is made of a mixture of nanomaterials and framework materials. And a composite film is formed by specific process steps such as mixing, stirring, suction filtration and baking, and then composited with the LiB alloy substrate.

Benefits of technology

It effectively suppresses the overflow of liquid metal lithium in LiB alloy, improves the overflow temperature of metal lithium, enhances the thermal stability and environmental adaptability of the thermal battery, and ensures a wider working temperature range and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003973423030000011
    Figure HDA0003973423030000011
  • Figure HDA0003973423030000012
    Figure HDA0003973423030000012
  • Figure HDA0003973423030000021
    Figure HDA0003973423030000021
Patent Text Reader

Abstract

The present invention discloses a LiB electrode material and a preparation method and application thereof. The LiB electrode material includes a LiB alloy substrate and an anti-overflow layer attached to the surface of the LiB alloy substrate, and the anti-overflow layer is made of a nanomaterial or a mixture of a skeleton material and a nanomaterial. In the present invention, the anti-overflow layer is prepared using a nanomaterial or a mixture of a skeleton material and a nanomaterial as a raw material, wherein the nanomaterial has a large adsorption capacity and capillary action that can achieve adhesion and blocking on the surface of the LiB alloy, thereby inhibiting the overflow of liquid metal lithium in the LiB alloy under high temperature and complex mechanical conditions. In addition, by providing an anti-overflow layer on the surface of the LiB alloy, the overflow temperature of the metal lithium of the LiB alloy negative electrode can be increased by about 50°C, which can help realize the research and development and manufacturing of thermal batteries with a wider temperature range under the premise of ensuring safety, and further improve the environmental adaptability of thermal batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal batteries, and in particular relates to a LiB electrode material and a preparation method and application thereof. Background Art

[0002] Thermal batteries have long storage time and are maintenance-free (storage time can reach 20 years), strong high current output capability (pulse current density can reach 10A cm -2 ), wide operating temperature range (-60℃~100℃), high reliability and other advantages are widely used in national defense, military and civilian fields. At present, lightweight and miniaturization are a major development trend of thermal batteries, and the development of high specific capacity thermal battery electrode materials has become a research hotspot.

[0003] Among the existing thermal battery products, LiB alloy is a very promising negative electrode material. Compared with traditional Li-Si alloy and Li-Al alloy negative electrodes, LiB alloy has higher specific capacity and stronger power characteristics, which is more conducive to the preparation of high energy density and high power density thermal batteries. However, LiB alloy has poor thermomechanical properties and there is a risk of metal lithium overflow under high temperature and complex mechanical environment. The outflow of liquid metal lithium may cause a short circuit in the battery, thereby causing thermal runaway of the battery. Since the thermomechanical properties of LiB alloy are closely related to the metal lithium content (the metal lithium content in LiB alloy determines the specific capacity), generally the higher the metal lithium content, the worse the thermomechanical properties. Therefore, the improvement of the specific capacity of LiB alloy often faces the problem that molten metal lithium is more likely to overflow. Summary of the invention

[0004] In view of the above-mentioned prior art, the present invention provides a LiB electrode material and a preparation method and application thereof, so as to solve the problem that LiB alloy is easy to overflow as an electrode material.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a LiB electrode material, including a LiB alloy substrate and an anti-overflow layer attached to the surface of the LiB alloy substrate; the anti-overflow layer is made of nanomaterials or a mixture of skeleton materials and nanomaterials.

[0006] Based on the above technical solution, the present invention can also be improved as follows.

[0007] Furthermore, the thickness of the anti-overflow layer is 0.005 mm to 0.2 mm.

[0008] Furthermore, the nanomaterial is at least one of a zero-dimensional nanomaterial, a one-dimensional nanomaterial and a two-dimensional nanomaterial.

[0009] Furthermore, the nanomaterial is at least one of nickel powder, silver powder, iron powder, copper powder, gold powder, cobalt powder, carbon powder, silicon carbide powder, graphene, carbon nanotubes and carbon fibers, and has a size of 10 nm to 200 μm.

[0010] Furthermore, the skeleton material is at least one of carbon fiber, carbon nanotube, nanosilver wire, nanogold wire, nanonickel wire, nanocopper wire, nanocobalt wire and nanosilicon carbide wire, and the diameter of the skeleton material is 2nm to 20μm, and the aspect ratio is greater than 500.

[0011] Further, the anti-overflow layer is prepared by the following steps:

[0012] S1: mixing the framework material and the nanomaterial in a mass ratio of 0 to 40:200, and then mixing the mixture with a solvent in a mass ratio of 1:2 to 100 to obtain a slurry;

[0013] S2: adding a soluble metal salt to the slurry to adjust the viscosity of the slurry to 50-500 mPa·S, and then stirring at a stirring speed of 500-3000 r / min for 5-120 min;

[0014] S3: diluting the slurry treated by S2 to a viscosity of 1 to 100 mPa·S, and then filtering at -1 to 0.01 MPa to obtain a composite film;

[0015] S4: Rinse the composite film 3 to 5 times with the solvent used in S1, and then bake it at 80 to 150° C. for 30 to 60 minutes.

[0016] Furthermore, the solvent is ethanol, acetone or deionized water; and the soluble metal salt is LiCl or NaCl.

[0017] The present invention also provides a method for preparing a LiB electrode material, the preparation method comprising the following steps:

[0018] S1: stacking the LiB alloy substrate on one side of the cut anti-overflow layer, wherein the edge of the anti-overflow layer exceeds the edge of the LiB alloy substrate by 0.1 to 0.5 mm;

[0019] S2: 5~100N / cm 2 The LiB alloy substrate and the anti-overflow layer are laminated together under a pressure of , and the anti-overflow layer is compounded with the LiB alloy substrate to obtain a product.

[0020] The invention also provides application of LiB electrode material in preparation of thermal battery.

[0021] Furthermore, the thermal battery is based on Fe 0.5 Co 0.5 S 2As the positive electrode, LiCl-KCl is used as the electrolyte, and LiB electrode material is used as the negative electrode.

[0022] The beneficial effects of the present invention are:

[0023] 1. In the present invention, the anti-overflow layer is prepared using nanomaterials or a mixture of skeleton materials and nanomaterials as raw materials. The large adsorption capacity and capillary action of the nanomaterials can achieve adhesion and blocking on the surface of the LiB alloy, thereby inhibiting the overflow of liquid metal lithium in the LiB alloy under high temperature and complex mechanical conditions.

[0024] 2. Under the same specific capacity conditions (lithium content), by setting an anti-overflow layer on the surface of the LiB alloy, the overflow temperature of the LiB alloy negative electrode to metallic lithium can be increased by about 50°C, which can help realize the research and development and manufacturing of thermal batteries with a wider temperature range while ensuring safety, and further improve the environmental adaptability of thermal batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a comparison chart of the thermal stability of sample A and sample B;

[0026] Figure 2 The discharge capacity comparison diagram of sample C and sample D;

[0027] Figure 3 These are cross-sectional images of the single-cell thermal batteries of sample C and sample D after discharge. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0029] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0030] The features and performance of the present invention are further described in detail below in conjunction with the examples. It is worth noting that the raw materials used in the present invention are all common commercial products, and their sources are not specifically limited.

[0031] Example 1

[0032] A LiB electrode material comprises a LiB alloy substrate and an anti-overflow layer attached to the surface of the LiB alloy substrate, wherein the thickness of the anti-overflow layer is 50 μm.

[0033] The LiB electrode material in this embodiment is prepared by the following steps:

[0034] (1) Preparation of anti-overflow layer

[0035] S1: Weigh 0.5 g of carbon nanotubes (diameter 10 nm, aspect ratio about 800) and 10 g of Ni powder (particle size 50 nm) into a 500 ml container, add 100 g of deionized water, and mix well to obtain a slurry;

[0036] S2: adding NaCl to the slurry to adjust the viscosity of the slurry to 100 mPa·S, and then stirring at a stirring speed of 1000 r / min for 60 min;

[0037] S3: dilute the slurry treated with S2 with deionized water to a viscosity of 10 mPa·S, and then form it through a vacuum filtration device with a vacuum degree of -0.5 MPa to obtain a composite film with a thickness controlled at 50 μm;

[0038] S4: The composite film is rinsed with deionized water for 4 times to remove NaCl inside the film; and then baked at 100° C. for 60 minutes to obtain an anti-overflow layer.

[0039] (2) Preparation of LiB electrode materials

[0040] The anti-overflow layer prepared above was cut into a disc with a diameter of 31 mm, and then the cut disc was attached to one side of a LiB alloy disc with a diameter of 30 mm, a thickness of 0.6 mm, and a lithium content of 65 wt% in a glove box with a water and oxygen content of less than 0.1 ppm. 2 The composite is pressed under pressure to obtain LiB electrode material.

[0041] Example 2

[0042] A LiB electrode material comprises a LiB alloy substrate and an anti-overflow layer attached to the surface of the LiB alloy substrate, wherein the thickness of the anti-overflow layer is 50 μm.

[0043] The LiB electrode material in this embodiment is prepared by the following steps:

[0044] (1) Preparation of anti-overflow layer

[0045] S1: Weigh 10g Ni powder (particle size 50nm) and place it in a 500ml container, add 100g deionized water, and mix well to obtain slurry;

[0046] S2: adding NaCl to the slurry to adjust the viscosity of the slurry to 100 mPa·S, and then stirring at a stirring speed of 1000 r / min for 60 min;

[0047] S3: dilute the slurry treated with S2 with deionized water to a viscosity of 10 mPa·S, and then form it through a vacuum filtration device with a vacuum degree of -0.5 MPa to obtain a composite film with a thickness controlled at 50 μm;

[0048] S4: The composite film is rinsed with deionized water for 4 times to remove NaCl inside the film; and then baked at 100° C. for 60 minutes to obtain an anti-overflow layer.

[0049] (2) Preparation of LiB electrode materials

[0050] The anti-overflow layer prepared above was cut into a disc with a diameter of 31 mm, and then the cut disc was attached to one side of a LiB alloy disc with a diameter of 30 mm, a thickness of 0.6 mm, and a lithium content of 65 wt% in a glove box with a water and oxygen content of less than 0.1 ppm. 2 The composite is pressed under pressure to obtain LiB electrode material.

[0051] Example 3

[0052] A LiB electrode material comprises a LiB alloy substrate and an anti-overflow layer attached to the surface of the LiB alloy substrate, wherein the thickness of the anti-overflow layer is 10 μm.

[0053] The LiB electrode material in this embodiment is prepared by the following steps:

[0054] (1) Preparation of anti-overflow layer

[0055] S1: Weigh 0.5 g of nanosilver wire (diameter 100 nm, aspect ratio about 1000) and 50 g of silver powder (particle size 100 nm) into a 500 ml container, add 100 g of ethanol, and mix well to obtain a slurry;

[0056] S2: Add LiCl to the slurry to adjust the viscosity of the slurry to 200 mPa·S, and then stir at a stirring speed of 3000 r / min for 5 min;

[0057] S3: dilute the slurry treated with S2 with ethanol to a viscosity of 50 mPa·S, and then form it through a vacuum filtration device with a vacuum degree of -1 MPa to obtain a composite film with a thickness controlled at 10 μm;

[0058] S4: The composite film is rinsed with ethanol 4 times to remove the LiCl inside the film; and then baked at 80°C for 60 minutes to obtain an anti-overflow layer.

[0059] (2) Preparation of LiB electrode materials

[0060] The anti-overflow layer prepared above was cut into a disc with a diameter of 31 mm, and then the cut disc was attached to one side of a LiB alloy disc with a diameter of 30 mm, a thickness of 0.6 mm, and a lithium content of 65 wt% in a glove box with a water and oxygen content of less than 0.1 ppm. 2 The composite is pressed under pressure to obtain LiB electrode material.

[0061] Example 4

[0062] A LiB electrode material comprises a LiB alloy substrate and an anti-overflow layer attached to the surface of the LiB alloy substrate, wherein the thickness of the anti-overflow layer is 5 μm.

[0063] The LiB electrode material in this embodiment is prepared by the following steps:

[0064] (1) Preparation of anti-overflow layer

[0065] S1: Weigh 10 g of cobalt powder (particle size 10 nm) and place it in a 500 ml container, add 100 g of deionized water, and mix well to obtain a slurry;

[0066] S2: adding NaCl to the slurry to adjust the viscosity of the slurry to 50 mPa·S, and then stirring at a stirring speed of 500 r / min for 120 min;

[0067] S3: dilute the slurry treated with S2 with deionized water to a viscosity of 10 mPa·S, and then form it through a vacuum filtration device with a vacuum degree of -1 MPa to obtain a composite film with a thickness controlled at 5 μm;

[0068] S4: The composite film is rinsed with deionized water for 4 times to remove NaCl inside the film; and then baked at 80° C. for 30 minutes to obtain an anti-overflow layer.

[0069] (2) Preparation of LiB electrode materials

[0070] The anti-overflow layer prepared above was cut into a disc with a diameter of 31 mm, and then the cut disc was attached to one side of a LiB alloy disc with a diameter of 30 mm, a thickness of 0.6 mm, and a lithium content of 65 wt% in a glove box with a water and oxygen content of less than 0.1 ppm. 2 The composite is pressed under pressure to obtain LiB electrode material.

[0071] Example 5

[0072] A LiB electrode material comprises a LiB alloy substrate and an anti-overflow layer attached to the surface of the LiB alloy substrate, wherein the thickness of the anti-overflow layer is 100 μm.

[0073] The LiB electrode material in this embodiment is prepared by the following steps:

[0074] (1) Preparation of anti-overflow layer

[0075] S1: Weigh 0.5 g of nano-cobalt wire (diameter 1 μm, long diameter about 600 mm) and 10 g of cobalt powder (particle size 1 μm) into a 500 ml container, add 100 g of acetone, and mix well to obtain a slurry;

[0076] S2: adding LiCl to the slurry to adjust the viscosity of the slurry to 500 mPa·S, and then stirring at a stirring speed of 3000 r / min for 60 min;

[0077] S3: dilute the slurry treated with S2 with acetone to a viscosity of 50 mPa·S, and then form it through a vacuum filtration device with a vacuum degree of -1 MPa to obtain a composite film with a thickness controlled at 100 μm;

[0078] S4: The composite film is rinsed with acetone 4 times to remove the LiCl inside the film; and then baked at 150° C. for 30 min to obtain an anti-overflow layer.

[0079] (2) Preparation of LiB electrode materials

[0080] The anti-overflow layer prepared above was cut into a disc with a diameter of 31 mm, and then the cut disc was attached to one side of a LiB alloy disc with a diameter of 30 mm, a thickness of 0.6 mm, and a lithium content of 65 wt% in a glove box with a water and oxygen content of less than 0.1 ppm. 2 The composite is pressed under pressure to obtain LiB electrode material.

[0081] Example 6

[0082] A LiB electrode material comprises a LiB alloy substrate and an anti-overflow layer attached to the surface of the LiB alloy substrate, wherein the thickness of the anti-overflow layer is 200 μm.

[0083] The LiB electrode material in this embodiment is prepared by the following steps:

[0084] (1) Preparation of anti-overflow layer

[0085] S1: Weigh 0.5 g of nano silicon carbide wire (diameter 10 μm, long diameter about 700) and 20 g of silicon carbide powder (particle size 10 μm) into a 500 ml container, add 100 g of deionized water, and mix well to obtain a slurry;

[0086] S2: adding LiCl to the slurry to adjust the viscosity of the slurry to 500 mPa·S, and then stirring at a stirring speed of 3000 r / min for 120 min;

[0087] S3: dilute the slurry treated with S2 with deionized water to a viscosity of 50 mPa·S, and then form it through a vacuum filtration device with a vacuum degree of -1 MPa to obtain a composite film with a thickness controlled at 200 μm;

[0088] S4: The composite film is rinsed with deionized water for 4 times to remove the LiCl inside the film; and then baked at 150° C. for 60 min to obtain an anti-overflow layer.

[0089] (2) Preparation of LiB electrode materials

[0090] The anti-overflow layer prepared above was cut into a disc with a diameter of 31 mm, and then the cut disc was attached to one side of a LiB alloy disc with a diameter of 30 mm, a thickness of 0.6 mm, and a lithium content of 65 wt% in a glove box with a water and oxygen content of less than 0.1 ppm. 2 The composite is pressed under pressure to obtain LiB electrode material.

[0091] Experimental Example 1

[0092] Since the LiB electrode materials prepared in Examples 2 to 4 have substantially the same performance as the LiB electrode material prepared in Example 1, the performance of the LiB electrode material is described by taking the LiB electrode material prepared in Example 1 (referred to as sample A) as an example.

[0093] In order to verify the improvement effect of the thermal stability of the LiB electrode material (sample A) in Example 1, a commercial untreated LiB alloy (sample B) of the same specification was used as a comparison to test the overflow degree of molten metal lithium. The test method was to clamp the sample to be tested with two stainless steel sheets and place it under constant temperature and constant pressure conditions of 500°C and 400N for 10 minutes. The test results are as follows: Figure 1 shown.

[0094] from Figure 1 It can be seen that under the test conditions, only a small amount of metallic lithium flows out from the edge of sample A (edge ​​point), while in sharp contrast, obvious traces of metallic lithium overflow appear at the edge of sample B, indicating that the molten metal lithium overflow of sample A is significantly better than that of sample B, indicating that the presence of the anti-overflow layer can effectively inhibit the overflow of molten metal lithium.

[0095] Experimental Example 2

[0096] A thermal battery was prepared using the LiB electrode material prepared in Example 1 as the negative electrode, and the positive electrode of the thermal battery was Fe 0.5 Co 0.5 S 2 The electrolyte of the thermal battery is LiCl-KCl (50wt% MgO), and the preparation method of the thermal battery is the same as that of the conventional single thermal battery. The prepared thermal battery is recorded as sample C. In addition, a thermal battery is prepared by using a commercial untreated LiB alloy of the same specification as the negative electrode, which is recorded as sample D. The positive electrode and electrolyte of sample D are the same as those of sample C.

[0097] The discharge performance of samples C and D was tested at 500°C and 400N with a current density of 0.2Acm -2 , the test results are as follows Figure 2 and 3 As shown. Figure 2 It can be seen that the discharge specific capacity of sample C is higher than that of sample D. The reason is that the negative electrode in sample C is a LiB alloy with an anti-overflow layer, which has better thermal stability and less metallic lithium overflow at 500°C. Figure 3 The cross-sectional photos of sample C and sample D after discharge show that there is no trace of metal lithium outflow at the edge of sample C, while there is obvious trace of metal lithium outflow at the edge of sample D. This shows that the presence of the anti-overflow layer can improve the thermal stability of the LiB alloy negative electrode and effectively inhibit the outflow of metal lithium under high temperature and extrusion environment.

[0098] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing a LiB electrode material, characterized in that: The following steps are involved: S1: stacking the LiB alloy substrate on one side of the cut anti-overflow layer, the edge of the anti-overflow layer exceeds the edge of the LiB alloy substrate by 0.1-0.5 mm; the anti-overflow layer is made of nanomaterials or a mixture of skeleton materials and nanomaterials; the nanomaterial is at least one of nickel powder, silver powder, iron powder, copper powder, gold powder, cobalt powder, carbon powder, silicon carbide powder, graphene, carbon nanotubes and carbon fibers; the skeleton material is at least one of carbon fibers, carbon nanotubes, nanosilver wires, nanogold wires, nanonickel wires, nanocopper wires, nanocobalt wires and nanosilicon carbide wires; S2: 5~100N / cm 2 The LiB alloy substrate and the anti-overflow layer are laminated together under a pressure of , and the anti-overflow layer is compounded with the LiB alloy substrate to obtain a product.

2. The method for preparing the LiB electrode material according to claim 1, characterized in that: The thickness of the anti-overflow layer is 0.005 mm to 0.2 mm.

3. The method for preparing the LiB electrode material according to claim 2, characterized in that: The nanomaterial is at least one of a zero-dimensional nanomaterial, a one-dimensional nanomaterial and a two-dimensional nanomaterial.

4. The method for preparing the LiB electrode material according to claim 3, characterized in that: The size of the nano material is 10nm~200μm.

5. The method for preparing the LiB electrode material according to claim 1, characterized in that: The diameter of the skeleton material is 2nm-20μm, and the aspect ratio is greater than 500.

6. The method for preparing the LiB electrode material according to any one of claims 1 to 5, characterized in that: The anti-overflow layer is prepared by the following steps: S1: mixing the framework material and the nanomaterial in a mass ratio of 0-40:200, and then mixing the mixture with the solvent in a mass ratio of 1:2-100 to obtain a slurry; S2: Add soluble metal salt to the slurry to adjust the viscosity of the slurry to 50-500 mPa·S, and then stir at a stirring speed of 500-3000 r / min for 5-120 min; S3: diluting the slurry treated by S2 to a viscosity of 1-100 mPa·S, and then filtering at -1-0.01 MPa to obtain a composite film; S4: Rinse the composite film 3 to 5 times with the solvent used in S1, and then bake it at 80 to 150°C for 30 to 60 minutes.

7. The method for preparing the LiB electrode material according to claim 6, characterized in that: The solvent is ethanol, acetone or deionized water; the soluble metal salt is LiCl or NaCl.

8. Use of the LiB electrode material prepared by the method for preparing the LiB electrode material according to any one of claims 1 to 7 in the preparation of a thermal battery.

9. The use according to claim 8, characterized in that: The thermal battery is based on Fe 0.5 Co 0.5 S2 is the positive electrode, LiCl-KCl is the electrolyte, and LiB electrode material is the negative electrode.