Elastomeric bicomponent fibers with unique feel
By using bicomponent fibers with an elastomeric core based on polypropylene and a non-elastomeric polyethylene skin, combined with secondary amide and pigment particles, the problem of insufficient drape and softness of elastic nonwoven mesh materials is solved, and non-adhesion is achieved properties and a cloth-like feel that enhances the fiber's spinnability and performance.
Patent Information
- Application Number
- CN202180032621.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-03-31
Smart Images

Figure CN115812086B_ABST
Abstract
Description
Background Art
[0001] Elastic or thermoplastic polymers, such as in the form of woven and nonwoven webs, are used in a variety of applications, examples of which include limited-use waistbands, side panels, leg pads and outer covers / backsheets, or disposable products including personal care absorbent articles. As known in the art, such articles may include children's and adult diapers, training pants, swimwear, incontinence garments, feminine hygiene products, funeral products, wound dressings, bandages, and the like. Elastic compositions may also be used in the field of protective covers, such as automotive, boat or other object coverings, tents (outdoor recreational coverings), agricultural fabrics (crop row coverings), and in veterinary and health care fields with products such as surgical drapes, hospital gowns, and fenestration reinforcements. In addition, such materials may also be used in other garments for cleanroom and health care environments.
[0002] For example, spunbond fabrics are formed from nonwoven webs and have proven useful in many different applications. While perfectly suitable for the above applications and others, existing nonwoven webs are known to have a plastic-like feel, making nonwovens less comfortable than more "clothing-like" fabrics because they often lack or have less drape, softness, and other tactile attributes, including a cool feel. For example, cloth has a more pleasing look and feel, as well as improved drape and softness, compared to plastic fabrics.
[0003] In addition, although elastic nonwovens such as spunbond fabrics have many uses, elastic fibers tend to self-stick, which is at least in part due to the low glass transition temperature (Tg) and high viscosity of the elastic polymer. This makes it difficult to form the fiber and lay down the nonwoven web because the elastic composition tends to stick between adjacent layers and adhere to the machine during fiber formation. In the past, attempts have been made to add an adhesion component to the outer layer or skin of a bicomponent fiber. However, it has been found that adhesion additives have failed to provide sufficient adhesion and spinnability properties to the fiber.
[0004] Therefore, it would be beneficial to provide an elastic spunbond that exhibits non-blocking properties. Additionally, it would be beneficial to provide a bicomponent elastic fiber to form a nonwoven web having good elastic properties and having a more cloth-like feel. It would be further beneficial to provide an elastic fiber for forming a nonwoven web such that the fiber and / or nonwoven web exhibits non-blocking properties and can be laminated to one or more additional layers. Summary of the invention
[0005] The present invention is generally directed to an elastomeric bicomponent fiber comprising a core and at least one sheath. The core comprises a polypropylene-based elastomer and a secondary amide, and the sheath comprises less than 50 weight percent of the total weight of the bicomponent fiber.
[0006] In one aspect, the polypropylene-based elastomer comprises an ethylene copolymer, an alpha-olefin copolymer, or a combination thereof. Additionally, in one aspect, the sheath comprises a non-elastomeric polymer. Additionally or alternatively, in one aspect, the sheath comprises a polyethylene polymer. Additionally, in one aspect, the polypropylene-based elastomer comprises a propylene / ethylene copolymer. Additionally, in one aspect, at least one sheath comprises 40 wt % or less of the total weight of the bicomponent fiber.
[0007] In another aspect, the secondary amide is present in the core in an amount of about 0.1% to about 10% by weight, based on the weight of the core. In another aspect, the secondary amide is present in the core in an amount of about 0.25% to about 5% by weight, based on the weight of the core. Additionally or alternatively, the secondary amide is a fatty acid amide. For example, in one aspect, the secondary amide has a structure of one of formulas (I)-(III):
[0008]
[0009] Where R 14 , R 15 , R 16 and R 18 Independently selected from C7-C 27 Alkyl groups and C7-C 27 an alkenyl group; and R 17 Selected from C8-C 28 Alkyl groups and C8-C 28 In another aspect, the secondary amide has the structure of formula (I), wherein R 14 It is CH2(CH2) 10 CH=CH(CH2)7CH3 and R 15 Yes -CH2(CH2) 15 CH3, or R 15 is CH2(CH2)6CH=CH(CH2)7CH3 and R 15 Yes -CH2(CH2) 13 CH3.
[0010] In addition, in one aspect, at least one of the sheath and the core further comprises pigment particles. In one aspect, the pigment particles are present in at least one of the sheath and the core in an amount of about 0.1 wt % to about 5 wt % based on the weight of the sheath or the core.
[0011] The present disclosure may also be directed to a spunbond nonwoven web as a whole, comprising an elastomeric bicomponent fiber having any one or more of the above aspects. In one aspect, the nonwoven web is post-bonded. In addition, in one aspect, the nonwoven web is perforated. In yet another aspect, the nonwoven web exhibits a cup compression peak load of about 20 grams-force (gf) based on a basis weight of about 48 grams per square meter (gsm).
[0012] Additionally or alternatively, the present disclosure also relates to a laminate as a whole, which includes a spunbond nonwoven web facing and a backing. The spunbond nonwoven web includes an elastomeric bicomponent fiber having a core and at least one sheath. The core comprises a polypropylene-based elastomer and a secondary amide, and the at least one sheath constitutes less than 50% by weight of the total weight of the bicomponent fiber. In one aspect, the backing is a film.
[0013] Furthermore, in one aspect, the present disclosure also generally includes an absorbent article formed from a nonwoven web or laminate having any one or more of the above aspects.
[0014] Other features and aspects of the invention are described in more detail below. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] A full and enabling disclosure of the present disclosure, including the best mode thereof, for one of ordinary skill in the art is more particularly described in the remainder of the specification with reference to the accompanying drawings, in which:
[0016] Figure 1 is a schematic diagram of an apparatus that may be used to form a spunbond nonwoven web material according to the present disclosure;
[0017] Figures 2A-2D Gray scale % coefficient of variation test is shown.
[0018] Repeat use of reference characters in the present specification and drawings is intended to represent same or analogous features or elements of the present disclosure. DETAILED DESCRIPTION
[0019] definition
[0020] As used herein, the terms "about", "approximately" or "substantially" when used to modify a value indicate that the value can be increased or decreased by 10% (e.g., such as 7.5%, 5%, such as 4%, such as 3%, such as 2%, such as 1%) and remain within the disclosed aspects. In addition, the term "substantially free" when used to describe the amount of a substance in a material is not limited to being completely or completely free, and can be equivalent to the lack of any perceptible or detectable amount of the listed substance in the material. Thus, for example, when the amount of a substance in a material is less than the precision of an industry-recognized instrument or test for measuring the amount of a substance in a material, the material is "substantially free" of the above-mentioned substance. In certain example embodiments, when the amount of a substance in a material is less than 10%, less than 9%, less than 8%, less than 7%, less than 6%, less than 5%, less than 4%, less than 3%, less than 2%, less than 1%, less than 0.5% or less than 0.1% by weight of the material, the material can be "substantially free" of the above-mentioned substance.
[0021] As used herein, the terms "elastomeric" and "elastic" refer to a material that can stretch in at least one direction (such as the CD or MD direction) upon application of a stretching force and contract / return to approximately its original dimensions upon release of the stretching force. For example, a stretched material may have a stretched length that is at least 50% greater than its relaxed, unstretched length and will return to within at least 50% of its stretched length upon release of the stretching force. A hypothetical example would be a one (1) inch sample of material that can be stretched to at least 1.50 inches and will return to a length of no more than 1.25 inches upon release of the stretching force. Advantageously, the material contracts or recovers at least 50% of the stretched length, and even more advantageously at least 80%.
[0022] As used herein, the term "fiber" generally refers to an elongated extrudate that can be formed by passing a polymer through a forming orifice such as a die. Unless otherwise indicated, the term "fiber" includes discontinuous fibers (e.g., stabilized fibers) and substantially continuous filaments having a certain length. Substantially continuous filaments may, for example, have a length much greater than their diameter, such as a length to diameter ratio ("aspect ratio") greater than about 15,000 to 1 and in some cases greater than about 50,000 to 1.
[0023] As used herein, the term "extensible" generally refers to a material that stretches or extends about 50% or more, in some aspects about 75% or more, in some aspects about 100% or more, and in some aspects about 200% or more of its relaxed length or width in the direction of an applied force (e.g., CD or MD direction).
[0024] As used herein, the term "nonwoven web" generally refers to a web having a structure of individual fibers or threads that are interlayered but not in an identifiable manner (such as in a knitted fabric). Examples of suitable nonwoven fabrics or webs include, but are not limited to, meltblown webs, spunbond webs, bonded carded webs, air-laid webs, coformed webs, hydroentangled webs, and the like.
[0025] As used herein, the term "meltblown web" refers broadly to a nonwoven web formed by a process in which a molten thermoplastic material is extruded as molten fibers through a plurality of fine, usually circular die capillaries into a converging high-velocity gas (e.g., air) stream that reduces the diameter of the fibers of the molten thermoplastic material to a microfiber diameter. Thereafter, the meltblown fibers are carried by the high-velocity gas stream and deposited on a collecting surface to form a web of randomly dispersed meltblown fibers. Such a process is, for example, known in the art. Butin et al. No. 3,849,241, which is incorporated herein by reference in its entirety for all purposes. Generally speaking, meltblown fiber webs can be substantially continuous or discontinuous microfibers that are generally less than 10 microns in diameter and are generally tacky when deposited onto a collecting surface.
[0026] As used herein, the term "spunbond web" generally refers to a web comprising substantially continuous fibers of small diameter. The fibers are formed by extruding molten thermoplastic material from a plurality of fine, usually circular capillaries of a spinneret having the diameter of the extruded fibers and then rapidly attenuating by, for example, eductive drawing and / or other well-known spunbond mechanisms. Spunbond webs are prepared, for example, in the patent application Appel et al. U.S. Patent No. 4,340,563, granted Dorschner et al. U.S. Patent No. 3,692,618, granted Matsuki et al. U.S. Patent No. 3,802,817, granted Kinney et al., U.S. Patent No. 3,338,992, Kinney et al., U.S. Patent No. 3,341,394, Hartman et al., U.S. Patent No. 3,502,763, Levy U.S. Patent No. 3,502,538, granted Dobo et al. U.S. Patent No. 3,542,615 and granted Pike et al. Spunbond fibers are described and illustrated in U.S. Patent No. 5,382,400 of , which is incorporated herein by reference in its entirety for all purposes. Spunbond fibers are generally not tacky when deposited onto a collecting surface. Spunbond fibers sometimes have a diameter of less than about 40 microns, and are typically between about 5 and about 20 microns.
[0027] As used herein, the term "coform" broadly refers to a composite material comprising a mixture or stabilized matrix of thermoplastic fibers and a second non-thermoplastic material. For example, a coform material can be made by a process wherein at least one meltblowing die is disposed adjacent a chute through which other materials are added to the web while the web is being formed. Such other materials can include, but are not limited to, fibrous organic materials such as wood or non-wood pulps such as cotton, rayon, recycled paper, pulp fluff, as well as superabsorbent particles, inorganic absorbent materials and / or organic absorbent materials, treated polymer staple fibers, and the like. Some examples of such coform materials are provided in the patent application Ser. Anderson et al. U.S. Patent No. 4,100,324, granted Everhart et al. U.S. Patent No. 5,284,703 and granted Georger et al., each of which is incorporated herein by reference in its entirety for all purposes.
[0028] As used herein, the term "thermal point bonding" generally refers to a process performed, for example, by passing a material between a patterned roll (e.g., a calendar roll) and another roll that may or may not be patterned (e.g., an anvil roll). One or both of the rolls are typically heated.
[0029] As used herein, the term "ultrasonic bonding" generally refers to a process performed, for example, by passing a material between an ultrasonic horn and a patterned roller (e.g., an anvil roller). For example, ultrasonic bonding performed using a stationary horn and a rotating patterned anvil roller is performed in a manner that grants Grgach et al. U.S. Patent No. 3,939,033, granted Rust Jr. U.S. Patent No. 3,844,869 and granted Hill The invention is described in U.S. Patent No. 4,259,399, which is incorporated herein by reference in its entirety for all purposes. In addition, ultrasonic bonding using a rotating horn and a rotating patterned anvil roll is described in U.S. Patent No. 4,259,399, which is incorporated herein by reference in its entirety for all purposes. Neuwirth et al. U.S. Patent No. 5,096,532, granted Ehlert U.S. Patent No. 5,110,403 and granted Brennecke et al. The invention is described in US Pat. No. 5,817,199, which is incorporated herein by reference in its entirety for all purposes. Of course, any other ultrasonic bonding technology may also be used in the present disclosure.
[0030] As used herein, "formation characteristics" or "gray level percent coefficient of variation" may be measured according to the following procedure:
[0031] Image analysis methods can be used to determine the formation characteristics of nonwovens and similar fiber webs. The method is usually implemented using transmitted light or incident light under a black background. The method used here adopts incident light under a black background, and a nonwoven sample is placed on the black background. Diffuse incident light illumination is provided by four LED floodlights placed above and around the sample, while allowing the camera to have enough spacing between them to observe the sample surface downward. Leica Microsystems DFC 310 camera is used and installed through c-mount, equipped with an adjustable Nikon 35-mm lens with an f-stop setting of 4. The camera and lens assembly are mounted on a Polaroid MP4 camera stand or equivalent at a distance above the sample that provides an image field size of about six inches wide. The camera is set to monochrome mode, and flat field correction is implemented on a white background before analysis.
[0032] The analysis is performed by placing the nonwoven sample on a camera stand or automatic sample stage (if available) and centering it under the optical axis of a Leica DFC 310 camera and a Nikon lens. The sample must be laid flat, and care must be taken to ensure that wrinkles or similar deformations are eliminated or avoided. An image analysis software package is used to monitor the illumination level, acquire the image, and then perform the measurement to determine the formation. For the analysis, the Leica Microsystems LAS software package is used to monitor the grayscale illumination of each sample between about 185 and 190 through an 8-bit grayscale system. The illumination level of the LED floodlight can be controlled via a common voltage controller equipped with a knob or slider for adjustment. Alternative software packages may also be used by those skilled in the art. Once the illumination level is adjusted and set, an image is acquired and saved to an analysis computer. The software is then used to measure the average grayscale level and grayscale standard deviation of the acquired image. The data is then electronically transferred to the analysis computer and saved in an EXCEL spreadsheet. One of the basic and main metrics of formation is the grayscale percentage coefficient of variation, or GL%COV for short. GL%COV is calculated as follows:
[0033] GL%COV=gray level standard deviation / average gray level×100%.
[0034] Each sample was analyzed at least 5 times. This was done by measuring five separate areas of each sample as described above. After the results were obtained, the samples could be compared to each other by performing basic statistical analysis, such as Student's T analysis at a 90% confidence level.
[0035] Detailed Description
[0036] Reference will now be made in detail to various aspects of the present disclosure, one or more examples of which are shown below. Each example is provided in an explanation rather than a limitation of the present disclosure. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present disclosure without departing from the scope or spirit of the present disclosure. For example, a feature illustrated or described as part of one aspect may be used in another aspect to produce yet another aspect. Therefore, the present disclosure is intended to encompass such modifications and variations.
[0037] In general, the present disclosure relates to a bicomponent fiber having improved spinnability and adhesion and an improved clothing-like feel. The bicomponent fiber contains a non-elastomeric polyethylene sheath and a polypropylene-based elastomeric core, wherein the core contains a secondary amide non-adhesive additive. Specifically, the present disclosure has surprisingly discovered that when a bicomponent fiber is formed according to the present disclosure, including when a secondary amide is included in the core along with an elastomeric polymer, the bicomponent fiber can still exhibit adhesion and textile properties while exhibiting a clothing-like feel even if a secondary amide adhesion additive is included in the core. Therefore, in one aspect, the sheath can be generally free of secondary amide adhesion additives.
[0038] For example, as measured using the cupping method discussed in more detail in the examples below, the bicomponent fiber according to the present disclosure may have improved softness. Specifically, the lower the peak load obtained from the cupping test, the softer the material. Therefore, in one aspect, the bicomponent fiber according to the present disclosure or the nonwoven formed therefrom may show about 100 grams of force (gf) or less, such as about 50gf or less, such as about 25gf or less, such as about 20gf or less, such as about 17.5gf or less, such as about 15gf or less, such as about 14gf or less cupping peak bending stiffness based on a basis weight of about 48gsm for a nonwoven web. The cupping peak load may also be reported as a value normalized by the sample basis weight. Thus, in one aspect, the bicomponent fibers and / or nonwoven webs formed therefrom can exhibit a strength of about 2.1 gf / gsm or less, such as about 2 gf / gsm or less, such as about 1.9 gf / gsm or less, such as about 1.8 gf / gsm or less, such as about 1.7 gf / gsm or less, such as about 1.6 gf / gsm or less, such as about 1.5 gf / gsm or less, such as about 1.4 gf / gsm or less, such as about 1.3 gf / gsm or less, such as about 1.2 gf / gsm or less. gf / gsm or less, for example about 0.4 gf / gsm or less, for example about 0.3 gf / gsm or less, for example about 0.25 gf / gsm or less of normalized cup compression peak load.
[0039] In addition, bicomponent fibers according to the present disclosure or nonwovens formed therefrom can also exhibit excellent puncture resistance, which indicates that the fibers have excellent material strength while remaining soft and elastic. Therefore, in one aspect, bicomponent fibers and / or nonwovens formed therefrom can exhibit a rupture peak load of about 900 gf or greater, such as about 925 gf or greater, such as about 950 gf or greater, such as about 975 gf or greater, such as about 1000 gf or greater, up to 1100 gf based on a nonwoven web having a basis weight of about 48 gsm. The rupture peak load can also be reported as a value normalized by the sample basis weight. Thus, in one aspect, the bicomponent fibers and / or nonwoven webs formed therefrom can exhibit a normalized peak load to burst of about 18 gf / gsm or greater, such as about 18.5 gf / gsm or greater, such as about 19 gf / gsm or greater, such as about 19.5 gf / gsm or greater, such as about 20 gf / gsm or greater, such as about 20.5 gf / gsm or greater, such as about 21 gf / gsm or greater, such as about 21.5 gf / gsm or greater, such as up to about 22 gf / gsm.
[0040] In addition, the present disclosure has also found that the bicomponent fibers also exhibit improved textile properties while maintaining good elastic and strength properties and a clothing-like feel. For example, as discussed above with respect to formation, the gray level (GL) % coefficient of variation (COV) is a quantitative measure of the uniformity or formation of the spunbond. Dark areas appear darker and light areas appear lighter, with each area assigned a gray level. The variation in gray levels of representative images of the spunbond acquired is then quantitatively evaluated to determine variations in local basis weight, and thus, lower gray level variations indicate a more uniform material. Thus, in one aspect, a spunbond formed using bicomponent fibers according to the present disclosure can exhibit a GL % COV of about 27.5% or less, such as about 27% or less, such as about 26.5% or less, such as about 26% or less, such as about 25.5% or less, such as about 25% or less, such as about 24.5% or less, based on a nonwoven web having a basis weight of about 17 gsm. In addition, as Figures 2A-2D , Figure 2A and 2C , which shows that a spunbond web formed from bicomponent fibers according to the present disclosure having a secondary amide in the core exhibits less variation (e.g., Figure 2B and 2D ).
[0041] In addition, the present disclosure has found that bicomponent fibers exhibit a cloth-like feel as demonstrated by improved thermal diffusivity, the measurement of which is described in the Examples below. For example, a bicomponent fiber may exhibit about 90 Ws 1 / 2 / m 2K or higher thermal conductivity, such as about 95Ws 1 / 2 / m 2 K or higher, e.g. about 100Ws 1 / 2 / m 2 K or higher, such as about 105Ws 1 / 2 / m 2 K or higher, e.g. about 110Ws 1 / 2 / m 2 K or higher, such as about 115Ws 1 / 2 / m 2 K or higher, e.g. about 120Ws 1 / 2 / m 2 K or higher, such as about 125Ws 1 / 2 / m 2 K or higher, e.g. about 130Ws 1 / 2 / m 2 K or higher, such as about 135Ws 1 / 2 / m 2 K or higher, e.g. about 150Ws 1 / 2 / m 2 K or higher, such as about 155Ws 1 / 2 / m 2 K or higher.
[0042] For example, in one aspect, the secondary amide can be a fatty acid amide, such as a suitable amide compound derived from the reaction between a fatty acid and ammonia or an amine-containing compound (e.g., a compound containing a primary or secondary amine group) to form a secondary amide. The fatty acid can be any suitable fatty acid, such as a saturated or unsaturated C8-C 28 Fatty acids, either saturated or unsaturated 12 -C 28 Fatty acids. In certain aspects, the fatty acids can be erucic acid (i.e., cis-13-docosaenoic acid), oleic acid (i.e., cis-9-octadecenoic acid), stearic acid (octadecanoic acid), behenic acid (i.e., behenic acid), arachidic acid (i.e., arachidic acid or eicosanoic acid), palmitic acid (i.e., hexadecanoic acid), and mixtures or combinations thereof. The amine-containing compound can be any suitable amine-containing compound, such as a fatty amine (e.g., stearylamine or oleylamine), ethylenediamine, 2,2′-iminodiethanol, and 1,1′-iminodipropan-2-ol.
[0043] In one aspect, the secondary amide can be a fatty acid amide having a structure of one of Formulas (I)-(III):
[0044]
[0045] in,
[0046] R 14 , R15 , R 16 and R 18 Independently selected from C7-C 27 Alkyl groups and C7-C 27 alkenyl groups, and in some aspects, C 11 -C 27 Alkyl groups and C 11 -C 27 an alkenyl group; and
[0047] R 17 Selected from C8-C 28 Alkyl groups and C8-C 28 alkenyl groups, and in some aspects, C 12 -C 28 Alkyl groups and C 12 -C 28 Alkenyl group.
[0048] For example, a fatty acid amide has the structure of formula (I), wherein R 14 Yes -CH2(CH2) 10 CH=CH(CH2)7CH3(erucamide) and R 15 Yes -CH2(CH2) 15 CH3, or R 15 is -CH2(CH2)6CH=CH(CH2)7CH3(oleamide) and R 15 Yes -CH2(CH2) 13 CH3. Similarly, in other aspects, the fatty acid amide can have a structure of formula (II), wherein R 16 It is CH2(CH2) 15 CH3 or -CH2(CH2)6CH=CH(CH2)7CH3. Secondary amides can also contain a mixture of two or more such fatty acid amides. However, in one aspect, such as the examples discussed below, the secondary amide additive is erucic acid amide, oleic acid amide, oleyl palmitamide, ethylenebisoleic acid amide, stearyl erucic acid amide or a combination thereof. Of course, it should be understood that in one aspect, the secondary amide can be a non-fatty acid amide.
[0049] Regardless of which secondary amide is selected, in one aspect, the secondary amide is present in the core in an amount of about 0.1 wt % to about 10 wt %, such as about 0.25 wt % to about 5 wt %, such as about 0.5 wt % to about 2.5 wt %, such as about 0.6 wt % to about 1.5 wt %, such as about 0.7 % to about 1 %, or any range or value therebetween, based on the weight of the core. Specifically, the disclosure has found that, surprisingly, the secondary amide in the core provides improved spinnability and non-blocking properties to the bicomponent fiber even when used in small amounts in the core.
[0050] Thus, in one aspect, the secondary amide can be present in the fiber in an amount of about 0.05% to about 8%, such as about 0.1% to about 4%, such as about 0.25% to about 2%, such as about 0.5% to about 1%, based on the weight of the fiber (e.g., the weight of the core + the weight of any sheath), or any range or value therebetween.
[0051] In one aspect, the secondary amide can generally be a low molecular weight secondary amide having a molecular weight of about 100 g / mol to about 1000 g / mol, such as about 200 g / mol to about 900 g / mol, such as about 300 g / mol to about 800 g / mol, such as about 400 g / mol to about 700 g / mol, or any range or value therebetween.
[0052] Despite the selection of secondary amides, the present disclosure has also found that while secondary amides can also improve the cloth-like feel of the fibers and the resulting nonwovens, the cloth-like feel of the fibers can be further improved by forming bicomponent fibers having at least one sheath formed of a non-elastomeric polyethylene, combined with an elastomeric core based on polypropylene, to provide an elastic fiber that exhibits improved non-blocking properties and a cloth-like feel. Thus, in one example, the bicomponent elastomeric fiber according to the present disclosure can exhibit elastic properties before and after being wound into a roll or bobbin, and can also have blocking properties that allow the fiber to be unwound from the roll or bobbin while maintaining a cloth-like feel. In addition, it has been found that excellent non-blocking properties are exhibited even when one or more sheaths constitute less than about 50% of the total weight of the elastomeric composition, such as about 45% or less, such as about 40% by weight or less, such as about 35% or less, such as about 30% or less, such as about 25% or less, such as about 20% or less, such as about 15% or less, such as about 10% or less.
[0053] Regardless of the number of skins, in one aspect, the elastomer that can be used for the core, skin, or both skin and core can be formed by one or more of a variety of thermoplastic elastomers and plastomer polymers, such as elastomeric polyesters, elastomeric polyurethanes, elastomeric polyamides, elastomeric copolymers, elastomeric polyolefins, etc. In a particular aspect, an elastomeric semi-crystalline polyolefin is used because of its unique combination of mechanical and elastomeric properties. Semi-crystalline polyolefins have or can show a substantially regular structure. For example, semi-crystalline polyolefins can be substantially amorphous in their undeformed state, but form crystalline domains when stretched. The crystallinity of olefin polymers can be from about 3% to about 60%, from about 5% to about 45% in some aspects, from about 10% to about 40% in some aspects, and from about 15% to about 35% in some aspects. Likewise, the semi-crystalline polyolefin may have a latent heat of fusion (ΔHf), which is another indicator of crystallinity, of from about 15 to about 210 joules per gram ("J / g"), in some aspects from about 20 to about 100 J / g, in some aspects from about 20 to about 65 J / g, and in some aspects from 25 to about 50 J / g. The semi-crystalline polyolefin may also have a Vicat softening temperature of from about 10°C to about 100°C, in some aspects from about 20°C to about 80°C, and in some aspects from about 30°C to about 60°C. The semi-crystalline polyolefin may have a melting temperature of from about 20°C to about 120°C, in some aspects from about 35°C to about 90°C, and in some aspects from about 40°C to about 80°C. The latent heat of fusion (ΔHf) is another indicator of crystallinity. f ) and melting temperatures can be measured using differential scanning calorimetry ("DSC") according to ASTM D-3417, as is well known to those skilled in the art. Vicat softening temperature can be measured according to ASTM D-1525.
[0054] Exemplary semi-crystalline polyolefins include polyethylene, polypropylene, and blends and copolymers thereof. In one particular aspect, the polyolefins used as ethylene and α-olefins (such as C3-C 20 α-olefins or C3-C 12Suitable α-olefins may be linear or branched (e.g., one or more C1-C3 alkyl branches, or aryl groups). Specific examples include 1-butene; 3-methyl-1-butene; 3,3-dimethyl-1-butene; 1-pentene; 1-pentene with one or more methyl, ethyl or propyl substituents; 1-hexene with one or more methyl, ethyl or propyl substituents; 1-heptene with one or more methyl, ethyl or propyl substituents; 1-octene with one or more methyl, ethyl or propyl substituents; 1-nonene with one or more methyl, ethyl or propyl substituents; 1-decene substituted with ethyl, methyl or dimethyl; 1-dodecene and styrene. Particularly desirable α-olefin comonomers are 1-butene, 1-hexene and 1-octene. Such copolymers may have an ethylene content of from about 60 mol% to about 99 mol%, in some aspects from about 80 mol% to about 98.5 mol%, and in some aspects from about 87 mol% to about 97.5 mol%. The alpha-olefin content may likewise be in the range of from about 1 mol% to about 40 mol%, in some aspects from about 1.5 mol% to about 15 mol%, and in some aspects from about 2.5 mol% to about 13 mol%.
[0055] The density of polyethylene can vary depending on the type of polymer used, but is generally between about 0.85 g / cm 3 To about 0.96g / cm 3 A polyethylene "plastomer" may, for example, have a density ranging from 0.85 g / cm 3 Up to 0.91g / cm 3 Similarly, a "linear low-density polyethylene" (LLDPE) may have a density ranging from about 0.91 g / cm 3 To about 0.94g / cm 3 range; "low density polyethylene" (LDPE) may have a density ranging from about 0.91 g / cm 3 To about 0.94g / cm 3 range; and "high density polyethylene" (HDPE) may have a density ranging from 0.94 g / cm 3 Up to 0.96g / cm 3 The density can be measured according to ASTM 1505.
[0056] Particularly suitable polyethylene copolymers are those that are "linear" or "substantially linear". The term "substantially linear" means that, in addition to short chain branches attributable to the incorporation of comonomers, the ethylene polymer also contains long chain branches in the polymer backbone. "Long chain branches" refers to a chain length of at least 6 carbons. Each long chain branch may have the same comonomer distribution as the polymer backbone and be as long as the polymer backbone to which it is attached. Preferred substantially linear polymers are substituted with 0.01 long chain branches per 1000 carbons to 1 long chain branch per 1000 carbons, and in some aspects substituted with 0.05 long chain branches per 1000 carbons to 1 long chain branch per 1000 carbons. In contrast to the term "substantially linear", the term "linear" means that the polymer lacks measurable or obvious long chain branches. That is, the polymer is substituted with less than 0.01 long chain branches per 1000 carbons on average.
[0057] The density of a linear ethylene / α-olefin copolymer is a function of both the length and amount of the α-olefin. That is, the greater the length of the α-olefin and the greater the amount of α-olefin present, the lower the density of the copolymer. Although not required, linear polyethylene "plastomers" are particularly desirable because the α-olefin short chain branching content makes the ethylene copolymer exhibit both plastic and elastomeric characteristics, i.e., "plastomers." Since polymerization with α-olefin comonomers reduces crystallinity and density, the resulting plastomers typically have a density lower than that of polyethylene thermoplastic polymers (e.g., LLDPE) but close to and / or overlapping elastomers. For example, the density of a polyethylene plastomer can be 0.91 g / cm 3 or less, in some aspects about 0.85 g / cm 3 To about 0.88g / cm 3 and in some aspects about 0.85 g / cm 3 To about 0.87g / cm 3 Although having densities similar to those of elastomers, plastomers generally exhibit a higher degree of crystallinity and can be formed into pellets that are non-sticky and relatively free-flowing.
[0058] The distribution of the alpha-olefin comonomer in the polyethylene plastomer is generally random and uniform among the different molecular weight fractions forming the ethylene copolymer. This uniformity of the comonomer distribution in the plastomer can be expressed as a comonomer distribution breadth index value ("CDBI") of 60 or greater, in some aspects 80 or greater, and in some aspects 90 or greater. In addition, the polyethylene plastomer can be characterized by a DSC melting point curve that exhibits a single melting point peak in the region of 50 to 110°C (second melt collapse).
[0059] Suitable plastomers for use in the present disclosure are those which may be designated EXACTTM Obtained from ExxonMobil Chemical Company of Houston, Texas, under the trade name ENGAGE TM and AFFINITY TM Ethylene-based copolymer plastomers available from Dow Chemical Company of Midland, Michigan, and under the trade name INFUSE TM , such as INFUSE TM 9807 is an olefin block copolymer available from Dow Chemical Company of Midland, Michigan. The polyethylene useful in the fibers of the present disclosure is DOW TM 61800.41. Other suitable ethylene polymers may be referred to as DOWLEX TM (LLDPE), ASPUN TM (LLDPE) and ATTANE TM (ULDPE) is available from The Dow Chemical Company. Other suitable ethylene polymers are available under the Ewen et al. U.S. Patent No. 4,937,299, granted Tsutsui et al. U.S. Patent No. 5,218,071, granted Lai et al. U.S. Patent No. 5,272,236 and granted Lai et al. No. 5,278,272 to , which is incorporated herein by reference in its entirety for all purposes.
[0060] However, it should be understood that in one aspect, one or more sheaths are formed from one or more ethylene polymers, such as one or more substantially non-elastomeric ethylene polymers. Thus, in one aspect, non-elastomeric polyolefins may include generally inelastic polymers such as conventional polyolefins (e.g., polyethylene, low density polyethylene (LDPE), Ziegler-Natta catalyzed linear low density polyethylene (LLDPE), etc., ultra low density polyethylene (ULDPE), polypropylene, polybutylene, etc.), polytetrafluoroethylene, polyesters (e.g., polyethylene terephthalate (PET), etc.), polyvinyl acetate, polyvinyl chloride-vinyl acetate, polyvinyl butyral, acrylic resins (e.g., polyacrylates, polymethyl acrylate, polymethyl methacrylate, etc.), polyamides (e.g., nylon), polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyurethane, polylactic acid, copolymers thereof, and mixtures thereof, and the like. For example, the sheath may include LLDPE available from Dow Chemical Co., Midland, Mich., such as DOWLEX TM 2517 or DOWLEXTM 2047 or a combination thereof, or Westlake Chemical Corp. of Houston, Tex. In addition, in one aspect, the non-adhesive polyolefin material can be other suitable ethylene polymers, such as those known by the names ASPUN™ (LLDPE) and ATTANE TM (ULDPE) available from Dow Chemical Company. Available from Dow Chemical Company under the name DOWLEX TM (LLDPE), ASPUN TM (LLDPE) and ATTANE TM (ULDPE).
[0061] Regardless of which polymers are selected for the one or more sheaths, the core may be formed from one or more semi-crystalline polyolefins as discussed above. For example, propylene polymers may also be suitable for use as semi-crystalline polyolefins. Suitable plastomer propylene polymers may include, for example, propylene copolymers or terpolymers, including propylene and α-olefins (e.g., C3-C 20 ) copolymers such as ethylene, 1-butene, 2-butene, various pentene isomers, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 4-methyl-1-pentene, 4-methyl-1-hexene, 5-methyl-1-hexene, vinyl cyclohexene, styrene, etc. The comonomer content of the propylene polymer can be about 35 wt% or less, in some aspects from about 1 wt% to about 20 wt%, and in some aspects from about 2 wt% to about 10 wt%. Preferably, the density of the polypropylene (e.g., propylene / α-olefin copolymer) can be 0.91 grams per cubic centimeter (g / cm 3 ) or less, in some aspects 0.85 to 0.88 g / cm 3 and in some aspects 0.85 g / cm 3 Up to 0.87g / cm 3 Suitable propylene-based copolymer plastomers may be referred to as VISTAMAXX TM (e.g., 2330, 6202, and 6102) (propylene-ethylene copolymer-based plastomers) are commercially available from ExxonMobil Chemical Co., Houston, Texas, under the name FINA TM (e.g., 8573) is commercially available from Atofina Chemicals, Feluy, Belgium, under the name TAFMER TM Commercially available from Mitsui Petrochemical Industries and under the name VERSIFY TMCommercially available from Dow Chemical Co. of Midland, Michigan. Other examples of suitable propylene polymers are given in Datta et al. U.S. Patent No. 6,500,563, granted Yang et al. U.S. Patent No. 5,539,056 and granted Resconi et al. No. 5,596,052, which is incorporated herein by reference in its entirety for all purposes.
[0062] However, it should be understood that in one aspect, the core is formed from a propylene polymer and / or copolymer. Thus, in one aspect, the core is formed from a propylene-based copolymer plastomer, such as that sold under the name VISTAMAXX TM Propylene-based copolymers (propylene-ethylene copolymer-based plastomers) are commercially available from ExxonMobil Chemical Co. of Houston, Texas (e.g., 2330, 6202, and 6102) under the name FINA TM (e.g., 8573) is commercially available from Atofina Chemicals of Feluy, Belgium, under the name TAFMER TM Commercially available from Mitsui Petrochemical Industries and under the name VERSIFY TM Commercially available from Dow Chemical Co. of Midland, Michigan.
[0063] Any of a variety of known techniques can generally be used to form semicrystalline polyolefins. For example, olefin polymers can be formed using free radical or coordination catalysts (e.g., Ziegler-Natta). Preferably, olefin polymers are formed by single-site coordination catalysts such as metallocene catalysts. Such catalyst systems produce ethylene copolymers in which the comonomers are randomly distributed within the molecular chain and uniformly distributed in the fractions of different molecular weights. Metallocene-catalyzed polyolefins are, for example, McAlpin et al. U.S. Patent No. 5,571,619, granted Davis et al. U.S. Patent No. 5,322,728, granted Obijeski et al. U.S. Patent No. 5,472,775, granted Lai et al. U.S. Patent No. 5,272,236 and granted Wheat et al.The U.S. Patent No. 6,090,325 of , which is incorporated herein by reference in its entirety for all purposes. The example of metallocene catalyst includes bis (n-butylcyclopentadienyl) titanium dichloride, bis (n-butylcyclopentadienyl) zirconium dichloride, bis (cyclopentadienyl) scandium chloride, bis (indenyl) zirconium dichloride, bis (methylcyclopentadienyl) titanium dichloride, bis (methylcyclopentadienyl) zirconium dichloride, cobalt, cyclopentadienyl titanium trichloride, ferrocene, hafnium dichloride, isopropyl (cyclopentadienyl-1-fluorenyl) zirconium dichloride, molybdenum dichloride, nickelocene, silver dichloride, ruthenocene, titanocene dichloride, hydrogen chloro zirconocene, zirconocene dichloride etc. The polymer made with metallocene catalyst generally has a narrow molecular weight range. For example, the polymer catalyzed by metallocene can have a polydispersity value (M) below 4. w / M n ), controlled short chain branching distribution, and controlled isotacticity.
[0064] The melt flow index (MI) of the semicrystalline polyolefin can generally vary, but is generally in the range of about 0.1 g / 10 min to about 100 g / 10 min, in some aspects about 0.5 g / 10 min to about 30 g / 10 min, and in some aspects about 1 to about 10 g / 10 min, these values are measured at 190° C. The melt flow index is the weight (in grams) of the polymer forced through an extrusion rheometer orifice (0.0825 inch diameter) when subjected to 5000 grams of force for 10 minutes at 190° C. and can be measured according to ASTM Test Method D1238-E.
[0065] Although core and sheath elastomers have been discussed thus far, it should be understood that the core and sheath may comprise the same elastomer or different elastomers. For example, in one aspect, the core may contain a polypropylene-based copolymer elastomer, such as a polypropylene / ethylene copolymer, as discussed above (e.g., VISTAMAXX TM AND / OR VERSIFY TM ), while the skin may contain a non-elastomeric polyethylene polymer (e.g., ASPUN TM ).
[0066] Nevertheless, as discussed above, the present disclosure has discovered that by including a non-elastomeric polyolefin material in combination with a core containing a propylene-based elastomer and a secondary amide, a non-blocked bicomponent fiber can be formed that exhibits a cloth-like feel and shows improved spinnability and adhesion even though the secondary amide is included in the core.
[0067] Although an elastomer is selected for the sheath and core, and / or a non-elastomeric polyolefin is selected for the sheath, a single polymer as described above may be used to form the elastomer and / or non-elastomeric polyolefin for the core, sheath, or both the core and sheath in an amount of up to 100 wt %, such as from about 75 wt % to about 99 wt %, such as from about 80 wt % to about 98 wt %, such as from about 85 wt % to about 95 wt %, based on the total weight of the nonwoven web material. However, in other aspects, the elastomer and / or non-elastomeric polyolefin may include two or more polymers from the above-mentioned polymers.
[0068] Furthermore, regardless of the elastomer and non-elastomeric polyolefin selected, in one aspect, the core is present in an amount from about 50 wt % to about 97.5 wt %, such as from about 60 wt % to about 95 wt %, such as from about 70 wt % to about 92.5 wt %, such as from about 80 wt % to about 90 wt %, such as from about 82.5 wt % to about 87.5 wt %, or any range or value therebetween, based on the total weight of the elastomeric composition.
[0069] In addition, in one aspect, in addition to or instead of the non-elastic polyolefin, the skin may also include one or more inorganic fillers. Thus, in one aspect, the skin includes one or more of calcium carbonate (CaCO3), various clays, silicon dioxide (SO2), aluminum oxide, barium sulfate, sodium carbonate, talc, magnesium sulfate, titanium dioxide, zeolite, aluminum sulfate, cellulose-type powder, diatomaceous earth, magnesium sulfate, magnesium carbonate, barium carbonate, kaolin, mica, carbon, calcium oxide, magnesium oxide, aluminum hydroxide, pulp powder, wood powder, cellulose derivatives, polymer particles, chitin, and chitin derivatives. In one aspect, the inorganic particles may include calcium carbonate, diatomaceous earth, or a combination thereof.
[0070] In one aspect, the skin, the core, or both the skin and the core can include pigment particles. In one aspect, the skin, the core, or both the skin and the core contain from about 0.1% to about 5% pigment particles based on the total weight of the skin, such as from about 0.5% to about 4.5%, such as from about 1% to about 4%, such as from about 1.5% to about 3.5%, or any range or value therebetween.
[0071] In addition, in one aspect, the skin, the core, or both the skin and the core can include a wetting agent to impart wettability to the bicomponent fiber. In this regard, based on the weight of the corresponding skin and / or core, the skin, the core, or both the skin and the core include about 10% by weight or less of the wetting agent, such as about 9% by weight or less, such as about 8% by weight or less, such as about 7% by weight or less, such as about 5% by weight or less, such as about 2.5% by weight or less. In one aspect, both the core and the skin can include a wetting agent according to the amount discussed above, but it should be understood that the above reference amount can also be about the total amount of the wetting agent in the skin and the core. In addition, in one aspect, the skin and the core do not contain a wetting agent.
[0072] Despite the selection of one or more final polymers and additives, the bicomponent fibers containing secondary amides according to the present disclosure can exhibit excellent properties. For example, in one aspect, based on a nonwoven web having a basis weight of about 48 gsm, the fibers according to the present invention can exhibit a hysteresis loss of about 80% or less, such as about 75% or less, such as about 72.5% or less, such as about 70% or less, such as about 67.5% or less, for which the test method is defined in more detail in the following examples, or any range or value therebetween.
[0073] In addition, the fibers can exhibit a 30% elongation of about 20% or less, such as about 17.5% or less, such as about 15% or less, such as about 12.5% or less, such as about 11% or less, based on a nonwoven web having a basis weight of about 48 gsm, as discussed in more detail in the examples below, or any range or value therebetween.
[0074] For example, in some aspects, the fiber can have a sheath-core arrangement, wherein the sheath can account for about 50% or less of the total weight of the fiber, such as about 45% or less, such as about 40% or less, such as about 35% or less, such as about 30% or less, such as about 25% or less, such as about 20% or less, such as about 15% or less, such as about 10% or less. In addition, in one aspect, the core can account for about 50% to about 97.5% by weight of the total weight of the fiber, such as about 60% to about 95% by weight of the total weight of the fiber, such as about 70% to about 92.5% by weight, such as about 80% to about 90% by weight, or any range or value therebetween.
[0075] Nevertheless, in one aspect, the present disclosure can generally also include forming a spunbond web using the elastomeric bicomponent fibers according to the present disclosure.
[0076] Regardless of the specific polymer used, a variety of techniques can generally be used to form a spunbond web formed by the elastomeric bicomponent fibers of the present disclosure. For example, in one aspect, the spunbond web can be formed by a spunbond process in which two or more polymer compositions are fed into an extruder and extruded through a conduit to a spinneret. Spinnerets for extruding fibers are well known to those skilled in the art. For example, a spinneret can include a housing containing a spin pack having a plurality of plates stacked on top of each other and having an opening pattern arranged to produce a flow path for the polymer composition. The spinneret can also have openings arranged in one or more rows that form a downwardly extruded fiber curtain when the polymer is extruded therefrom. The process can also employ a quench blower positioned adjacent to the fiber curtain extending from the spinneret. Air from the quench blower quenches the fibers as they are formed. A fiber drafting unit or aspirator can also be positioned below the spinneret to receive the quenched fibers. Fiber drafting units or aspirators for melt-spinning polymers are well known in the art. The fiber drawing unit may include an elongated vertical channel, and fibers are drawn from the channel by suction air entering from the side of the channel and flowing downward through the channel. A heater or a blower may supply suction air to the fiber drawing unit, and the fiber drawing unit draws the fibers and ambient air therethrough.
[0077] Generally, the resulting fibers have an average size (e.g., diameter) of about 100 microns or less, in some aspects about 0.1 microns to about 50 microns, such as about 0.5 microns to about 40 microns, such as about 1 micron to about 30 microns, such as about 2.5 microns to about 20 microns, or any range or value therebetween.
[0078] Regardless of the form of the spunbond web, additives may also be incorporated into the spunbond web or fibers formed therefrom, such as melt stabilizers, processing stabilizers, heat stabilizers, light stabilizers, antioxidants, heat aging stabilizers, brighteners, antiblocking agents, viscosity modifiers, and the like. Viscosity modifiers may also be used, such as polyethylene waxes (e.g., EPOLENE from Eastman Chemical). TM C-10). Phosphite stabilizers (e.g., IRGAFOS available from Ciba Specialty Chemicals of Tarrytown, NY and DOVERPHOS available from Dover Chemical Corp. of Dover, Ohio) are exemplary melt stabilizers. In addition, hindered amine stabilizers (e.g., CHIMASSORB available from Ciba Specialty Chemicals) are exemplary heat and light stabilizers. In addition, hindered phenols are commonly used as antioxidants in film manufacturing. Some suitable hindered phenols include those available under the trade name IRAGANOX TM Such as IRGANOXTM 1076, 1010 or E 201 are available from Ciba Specialty Chemicals. When employed, such additives (e.g., antioxidants, stabilizers, etc.) can each be present in an amount of about 0.001% to about 25% by weight of the nonwoven web material, in some aspects about 0.005% to about 20% by weight, and in some aspects 0.01% to about 15% by weight.
[0079] Reference Figure 1 , various aspects of the fiber formation process will be discussed. Figure 1 , for example, illustrates in greater detail one aspect of a process for forming fibers that may be used in the present disclosure. Although by no means required, Figure 1 The process shown in is configured to form a substantially continuous bicomponent fiber with an A / B configuration. More specifically, polymer compositions A and B are initially supplied to a fiber spinning device 21 to form a bicomponent fiber 23. Once formed, the fiber 23 passes through a fiber drafting unit 25 and is deposited on a moving forming wire 27. The deposition of the fiber is assisted by a vacuum below the wire provided by a suction box 29, which pulls the fiber 23 downward onto the forming wire 27. The forming wire 27 is porous so that the vertical air flow formed by the suction box 29 can cause the fiber to fall. In one aspect of the present disclosure, the flow rate of the air flow can be kept relatively low to enhance the tendency of the fiber 23 to remain oriented in the MD direction. Alternatively, the suction box may include a section extending in the longitudinal direction to destroy the vertical air flow where the fiber falls onto the moving net, so that the fiber can have a higher degree of longitudinal orientation. An example of such a technology is described in, for example, U.S. Patent No. 6,331,268. Of course, other technologies can also be used to help the fiber remain oriented in the longitudinal direction. For example, a deflector guide plate or other mechanical element may be used, such as described in U.S. Patent Nos. 5,366,793 and 7,172,398. The direction of the air flow used to thin the fibers when forming the fibers may also be used to adjust to achieve longitudinal orientation, such as described in U.S. Patent No. 6,524,521. In addition to the above process, other known techniques may also be used to form the fibers. In one aspect, for example, the fibers may be quenched after they are formed and then deposited directly on the forming wire without first being drafted in the above manner. In such aspects, as described above, the flow rate of such airflow may be kept relatively low to enhance the orientation of the fibers to maintain orientation in the MD direction, however, it should be understood that in one aspect, the fibers are not primarily oriented in the MD direction.
[0080] See again Figure 1Once the fibers 23 are formed, they can be heated by a diffuser 33, which can blow hot air onto the fiber surface to gently bond them together for further processing. A hot air knife can also be used as an alternative to a diffuser. Other techniques for integrating the web, such as heated calendering rollers, can also be used. In any case, the resulting fibers can then be bonded to form a consolidated, coherent nonwoven web structure. Any suitable bonding technique can generally be used in the present disclosure, such as adhesives or spontaneous bonding (e.g., fusion and / or self-bonding of fibers without applying external adhesives). Spontaneous bonding can be achieved, for example, by contacting the fibers when they are semi-molten or tacky, or simply by blending a tackifying resin and / or solvent with a polymer composition for forming the fibers. Suitable spontaneous bonding techniques can include ultrasonic bonding, thermal bonding, air penetration bonding, and the like. Hot spot bonding, for example, generally uses a roller gap formed between two rollers, at least one of which is patterned. On the other hand, ultrasonic bonding generally uses a gap formed between an ultrasonic horn and a patterned roller.
[0081] The specific properties of bonding pattern can be changed as needed. A suitable bonding pattern is, for example, called "S-shaped braiding" pattern, and is described in U.S. Patent No. 5,964,742 to McCormack et al. Another suitable bonding pattern is called "rib knitting" pattern and is described in U.S. Patent No. 5,620,779 to Levy et al. Another suitable pattern is "wire braiding" pattern, which has about 200 to about 500 bonding sites per square inch and about 250 to about 350 bonding sites per square inch in some aspects. Of course, other bonding patterns can also be used, such as U.S. Patent No. 3,855,046 to Hansen et al., U.S. Patent No. 5,962,112 to Haynes et al., U.S. Patent No. 6,093,665 to Sayovitz et al., D375,844 to Edwards et al., D428,267 to Romano et al. and D390,708 to Brown. In addition, bonding patterns can also be used that include bonding areas that are generally oriented in the machine direction and have an aspect ratio of about 2 to about 100, in some aspects about 4 to about 50, and in some aspects about 5 to about 20. The pattern of bonding areas is also typically selected so that the total bond area of the spunbond fiber web is less than about 50% (determined by conventional optical microscopy methods), in some aspects, less than about 30%, such as less than about 25%, such as less than about 20%, such as less than about 17.5%.
[0082] Regardless of the type of nonwoven web material formed, the basis weight of the nonwoven web material can generally vary, such as from about 8 grams per square meter ("gsm") to about 150 gsm, in some aspects from about 15 gsm to about 125 gsm, and in some aspects from about 25 gsm to about 100 gsm. When multiple nonwoven web materials are used, such materials can have the same or different basis weights.
[0083] The spunbond web may also be subjected to one or more additional post-processing steps, as is known in the art. For example, the spunbond web may be stretched in the cross direction using known techniques such as tenter stretching, groove roll stretching, etc. The spunbond web may also be subjected to other known processing steps, such as perforation, heat treatment, etc.
[0084] In one aspect, a spunbond web formed using elastomeric bicomponent fibers according to the present disclosure may form all or a portion of a composite nonwoven fabric. Of course, it should also be understood that the nonwoven fabric may include additional layers (e.g., nonwoven webs, films, strands, etc.) if additional layers are desired. For example, the fabric may include two (2) or more layers and in some aspects three (3) to ten (10) layers (e.g., 3 or 5 layers). In one aspect, for example, the nonwoven fabric may include an inner nonwoven layer (e.g., meltblown or spunbond) positioned between two outer nonwoven layers (e.g., spunbond). For example, the inner nonwoven layer may be formed from a spunbond web of the present disclosure, and one or both of the outer nonwoven layers may be formed from a spunbond web of the present disclosure or a conventional nonwoven web. Alternatively, the inner nonwoven layer may be formed from a spunbond web of the present disclosure or a conventional nonwoven web, and one or both of the outer nonwoven layers may be formed from a spunbond web of the present disclosure. Various techniques for forming laminates having this property are described in the grant. Brock et al. U.S. Patent No. 4,041,203, granted Timmons et al. U.S. Patent No. 5,213,881, granted Timmons et al. U.S. Patent No. 5,464,688, granted Bornslaeger U.S. Patent No. 4,374,888, granted Collier et al. U.S. Patent No. 5,169,706 and granted Brock et al. The facings may have other constructions and any desired number of layers, such as spunbond / meltblown / meltblown / spunbond ("SMMS") laminates, spunbond / meltblown ("SM") laminates, and the like.
[0085] Regardless of the method of forming the spunbond nonwoven web or the number of layers in the facestock, in one aspect, the nonwoven facestock can be used in a laminate by laminating the nonwoven facestock to an elastic film or other backing or any other layer as described above. Lamination can be achieved using a variety of techniques, such as adhesive bonding, thermal point bonding, ultrasonic bonding, etc. as described above. The specific bonding pattern is not critical to the present disclosure, and any of the bonding patterns, hole formation, and stretching discussed above with respect to spunbond webs can also be used for lamination. However, in one aspect, the above-mentioned laminate can have improved biaxial stretch and / or bending length properties by means of an elastomeric film and an extensible (or elastomeric) nonwoven web material formed from bicomponent fibers according to the present disclosure and a lamination method.
[0086] For example, in one aspect, a stretch ratio of about 1.5 or greater, or 2 to 6, or 2.5 to 7.0, or 3.0 to 5.5 is used to achieve a desired degree of tension in the film during lamination. The stretch ratio can be determined by dividing the final length of the film by its original length. The stretch ratio can be roughly the same as the draft ratio, which can be determined by dividing the linear speed of the film during lamination (e.g., the speed of the nip roll) by the linear speed of the film formation (e.g., the speed of the casting roll or the blow molding nip roll).
[0087] Whether laminated to a backing or used alone as a nonwoven web, spunbond webs can be used in a variety of applications. For example, as described above, spunbond webs can be used in absorbent articles. "Absorbent article" generally refers to any article capable of absorbing water or other fluids. Examples of some absorbent articles include, but are not limited to, personal care absorbent articles, such as diapers, training pants, absorbent underpants, incontinence products, feminine hygiene products (e.g., sanitary napkins, panty liners, etc.), swimsuits, baby wipes, etc.; medical absorbent articles, such as clothing, fenestration materials, pads, mattresses, bandages, absorbent drapes, and medical wipes; food service wipers; clothing; etc., and can be uniquely positioned for wearable articles due to its improved clothing-like feel.
[0088] Several examples of such absorbent articles are given in DiPalma et al. U.S. Patent No. 5,649,916, granted Kielpikowski U.S. Patent No. 6,110,158 and granted Blaney et al. Other suitable products are described in the patent No. 6,663,611 of Fell et al. U.S. Patent Application Publication No. 2004 / 0060112 A1 and Grant No. Damico et al. U.S. Patent No. 4,886,512, granted Sherrod et al. U.S. Patent No. 5,558,659, granted Fell et al. U.S. Patent No. 6,888,044 and granted Freiburger et al.The absorbent articles of the present invention are described in U.S. Pat. No. 6,511,465. The materials and processes for forming such absorbent articles are well known to those skilled in the art. Typically, absorbent articles include a substantially liquid-impermeable layer (e.g., outer cover), a liquid-permeable layer (e.g., body side liner, surge layer, etc.), and an absorbent core. In a particular aspect, the composite materials disclosed herein can be used to provide a waist portion, leg cuffs / pads, ears, side panels, or outer coverings.
[0089] The present invention may be better understood by reference to the following examples.
[0090] Test Method
[0091] With the exception of the GL %COV described above which is based on a nonwoven web having a basis weight of about 17 gsm, all properties tested in the Examples are reported based on a nonwoven web having a basis weight of about 48 gsm.
[0092] Bursting strength
[0093] Burst strength is a measure of the ability of a fiber structure to absorb energy when deformed perpendicular to the plane of the fiber structure. Burst strength can be measured in accordance with ASTM D-6548, except that the test is conducted on a constant rate extension type (MTS Systems Corporation, Eden Prairie, Minn.) tensile tester with computer-based data acquisition and frame control system, wherein the dynamometer is positioned above the sample fixture so that the penetrating member is lowered into the test sample, causing it to rupture. The dynamometer and sample are arranged in the same manner as in ASTM D-6548. Figure 1 The penetration assembly consists of a hemispherical anodized aluminum penetration member having a diameter of 1.588 ± 0.005 cm, which is fixed to an adjustable rod with a ball-ended socket. The test specimen is fixed in a specimen clamp consisting of upper and lower aluminum concentric rings between which the specimen is firmly fixed by mechanical clamping during testing. The specimen clamping ring has an inner diameter of 8.89 ± 0.03 cm.
[0094] The tensile tester was set up so that the crosshead speed was 15.2 cm / min, the probe spacing was 104 mm, the break sensitivity was 60%, the relaxation compensation was 10 gf, and the instrument was calibrated according to the manufacturer's instructions.
[0095] The samples were conditioned under TAPPI conditions and cut into squares of 127×127 mm±5 mm. For each test, a total of 3 product sheets were combined. The sheets were stacked on top of each other in such a way that they were aligned longitudinally. In the case where the sample contained multiple plies, the plies were not separated for testing. In each case, the test sample contained 3 product sheets. For example, if the product is a 2-ply tissue product, 3 product sheets were tested, for a total of 6 plies. If the product is a single-ply tissue product, 3 product sheets were tested, for a total of 3 plies.
[0096] Before testing, adjust the probe height if necessary by inserting the rupture fixture into the bottom of the tensile tester and lowering the probe until it is positioned approximately 12.7 mm above the alignment plate. Then adjust the probe length until the probe rests in the recessed area of the alignment plate when lowered.
[0097] It is recommended to use a dynamometer where the majority of the peak load results fall between 10% and 90% of the dynamometer range. To determine the most appropriate dynamometer for testing, initially test the sample to determine the peak load. If the peak load is < 450 gf, use a 10 Newton dynamometer, if the peak load is > 450 gf, use a 50 Newton dynamometer.
[0098] Once the equipment has been set up and the force gauge selected, the sample is tested by inserting it into the sample clamps and holding the test sample in place. The test sequence is then initiated, causing the penetration assembly to descend at the rate and distance specified above. When the test sample ruptures under the action of the penetration assembly, the measured penetration force resistance is displayed and recorded. The sample clamps are then released, the sample is removed, and the equipment is ready for the next test.
[0099] The peak load (gf) and peak energy (g-cm) were recorded.
[0100] Softness / cup compression test:
[0101] The softness of a nonwoven fabric can be measured according to the "cup compression" test. The cup compression test evaluates the stiffness of a fabric by measuring the peak load (also called the "cup compression load" or just "cup compression") and the energy required to crush the sample, and in turn quantifies the softness of the sample. The sample is placed in a forming cup. The forming cup and sample are then placed on a load plate mounted on a tensile tester. A presser foot is lowered through the open end of the forming cup and "crushes" and distorts the cup-shaped sample inside. The maximum load measured in grams-force (gf) and the energy measured in grams-force-length (gf-mm) are the results. The results are an indication of the stiffness of the material. The stiffer the material, the higher the peak load and energy values. The softer the material, the lower the values.
[0102] The constant rate of extension tensile tester is equipped with a computerized data acquisition system (e.g., MTS TestWorks for Windows Version 4, from MTS Systems Corporation, Eden Prairie, Minn. 55344-2290) that is capable of calculating peak load and energy between two predetermined distances (15-60 mm) in compression mode, preferably at a minimum data capture rate of 20 data points per second. A suitable device for measuring compression cup deformation is a Model FTD-G-500 dynamometer (500 gram range) available from Schaevitz Company, Pennsauken, NJ, and tensile testers and dynamometers available from Instron Corporation, Canton, Mass. 02021 or Sintech, Inc., PO Box 14226, Research Triangle Park, NC 27709-4226.
[0103] The energy measured is the energy required for a hemispherical presser foot of 4.5 cm diameter to crush a 23 cm x 23 cm piece of fabric into an inverted cup of about 6.5 cm diameter x 6.5 cm high, while the cup-shaped fabric is surrounded by a cylinder (forming cup) of about 6.5 cm diameter to maintain uniform deformation of the cup-shaped fabric during the test. The average of 3-5 readings is used. The test is conducted in a standard laboratory atmosphere of 23 ± 2 ° C and 50 ± 5% relative humidity. Before testing, the material should be allowed to reach ambient temperature. The sample is prepared by placing a retaining ring on the forming table. The material is then placed on the forming table. The forming cup is placed on the sample and the forming table to conform the sample to the cup shape. The retaining ring engages with the forming cup to secure the sample in the forming cup. The forming cup is removed, and the now formed sample inside is removed at the same time. The sample is secured in the forming cup by the retaining ring. The sample, forming cup and retaining ring are inverted and placed in the tensile tester. The presser foot and the forming cup are aligned in the tensile tester to avoid contact between the cup wall and the presser foot, which would affect the reading. A presser foot (0.5 inch, made of lightweight nylon or metal) passes through an opening in the bottom of an inverted forming cup to crush the cup-shaped sample inside. The peak load is measured when the presser foot descends at a rate of approximately 406 mm per minute and is measured in grams. The cup compression test also produces a value for the total energy required to squeeze the sample ("cup compression energy"), which is the energy from the start of the test to the peak load point, i.e., the area under the curve formed by the load in grams on one axis and the distance the presser foot moves in millimeters on the other axis. Therefore, the cup compression energy is reported in gf-mm. A lower cup compression value indicates a softer laminate.
[0104] Multi-cycle stress / strain testing of raw materials
[0105] The multi-cycle stress / strain test is a two-cycle elongation and recovery test used to measure the elongation and recovery characteristics of elastomeric raw materials and elastomeric composites. In particular, the test can be used to determine what effect, if any, the application of the formulation to a substrate has on its elongation and recovery characteristics. Deterioration of substrate properties measured by this test is manifested as loss of tension or deterioration of elongation resistance, which can result in extreme elongation when force is applied, such as sagging.
[0106] This test measures the load value of a test sample placed under a specific amount of strain (e.g., stretched to a specific elongation). Such load values are determined during both the elongation and recovery phases of the test and during each of the two cycles. For this example, the load value was set at 30% elongation. Generally, a decrease in the amount of load retained after treatment indicates a negative impact on the elastic characteristics of the substrate, even in the absence of significant degradation or delamination of the substrate.
[0107] Hysteresis is a measure of how well an elastic material retains its elastic properties after multiple stretches. It is the loss of mechanical energy that occurs during loading and unloading cycles, and it is shown by the area between the loading and unloading curves. The lower the hysteresis loss, the more the NBL / EMC retains its elastic behavior and the more it acts like a rubber band. This is critical in diaper fit performance to ensure that the ears can do their fastening job even after multiple stretches.
[0108] Percent set is the permanent deformation caused by the load. Because the NBL / EMC material loses some energy when it is stretched, it will not return to exactly 0 grams when the retraction cycle returns to 0% elongation. The lower the percent set, the better the elastic properties and the material behaves more like a rubber band, which helps with conformability.
[0109] Strip tensile peak load
[0110] After elongation is complete, the sample is held between grips having front and back faces of 25.4 mm x 76 mm. The grip faces are rubberized with the longer dimension of the grips being perpendicular to the pulling direction. The grip pressure is pneumatically maintained at a pressure of 40 pounds per square inch. The tensile test is conducted at a rate of 300 mm per minute, with a gauge length of 76 mm and a break sensitivity of 40%.
[0111] Three samples were tested by applying the test load in the machine direction and three samples were tested by applying the test load in the cross direction. In addition to tensile strength, peak load, peak stretch (i.e., % elongation at peak load) and peak energy were measured. The peak strip tensile loads of each test sample were averaged to determine MD or CD tensile strength.
[0112] Diffusion rate
[0113] According to ASTM D7984-16 (“Test Method for Measurement of Thermal Effusivity of Fabrics Using a Modified Transient Plane Source (MTPS) Instrument”), the thermal diffusivity of the sample was measured using a C-Therm TCi thermal conductivity analyzer.
[0114] The default C-Therm TCi thermal conductivity analyzer uses a modified transient plane source (MTPS) technique when characterizing the thermal conductivity and diffusivity of materials. It uses a single-sided interface thermoreflectance sensor that applies an instantaneous constant heat source to the sample.
[0115] Example 1
[0116] The spunbond nonwoven web was formed using bicomponent fibers having the core components shown in Table 1 (note the PE 3 The samples have a single component arrangement and are formed only by the PE). The skin is 100% Dow 6840A ethylene polymer. After forming, the spunbond webs were subjected to various tests for strength, elasticity, softness and spinnability, the results of which are shown in Table 1.
[0117] Table 1
[0118]
[0119]
[0120] 1-EXXON Mobile 3155 non-elastic polypropylene
[0121] 2- A concentrate containing 15% by weight of a secondary amide as described above, with an active amount of 0.75% by weight of the secondary amide in the core
[0122] 3-Dow 6840A Ethylene polymer (skin composition, no core)
[0123] 4-VISTAMAXX Elastic Polypropylene Copolymer
[0124] Although the present disclosure has been described in detail with respect to certain aspects of the present disclosure, it will be appreciated that those skilled in the art, after obtaining an understanding of the foregoing, can easily conceive of changes, variations and equivalents to these aspects. Therefore, the scope of the present disclosure should be assessed as the scope of the appended claims and any equivalents thereof.
Claims
1. An elastomeric bicomponent fiber comprising: a core comprising a polypropylene-based elastomer and a secondary amide; and at least one sheath, the at least one sheath being free of secondary amides; wherein said at least one sheath constitutes less than 50 weight percent of the total weight of said bicomponent fiber; wherein the sheath comprises a polyethylene polymer, the secondary amide is present in the core in an amount of 0.1% to 10% by weight based on the weight of the core, and the secondary amide is a fatty acid amide.
2. The elastomeric bicomponent fiber of claim 1, wherein the polypropylene-based elastomer comprises an ethylene copolymer, an α-olefin copolymer, or a combination thereof.
3. The elastomeric bicomponent fiber of claim 1 or 2, wherein the sheath comprises a non-elastomeric polymer.
4. The elastomeric bicomponent fiber of claim 1 or 2, wherein the secondary amide is present in the core in an amount of 0.25% to 5% by weight based on the weight of the core.
5. The elastomeric bicomponent fiber of claim 1 or 2, wherein the secondary amide has a structure of one of formulas (I) to (III): in, R 14 , R 15 , R 16 and R 18 Independently selected from C7-C 27 Alkyl groups and C7-C 27 an alkenyl group; and R 17 Selected from C8-C 28 Alkyl groups and C8-C 28 Alkenyl group.
6. The elastomeric bicomponent fiber of claim 5, wherein the secondary amide has a structure of formula (I), wherein R 14 Yes -CH2(CH2) 10 CH=CH(CH2)7CH3 and R 15 Yes -CH2(CH2) 15 CH3, or R 15 is -CH2(CH2)6CH=CH(CH2)7CH3 and R 15 Yes -CH2(CH2) 13 CH 3。 7. The elastomeric bicomponent fiber of claims 1 or 2, wherein the polypropylene-based elastomer comprises a propylene / ethylene copolymer.
8. The elastomeric bicomponent fiber of claims 1 or 2, wherein the core comprises a second elastomer.
9. The elastomeric bicomponent fiber of claims 1 or 2, wherein pigment particles are present in at least one of the sheath and core in an amount of 0.1% to 5% by weight based on the weight of the sheath or the core.
10. The elastomeric bicomponent fiber of claim 1 or 2, wherein the at least one sheath comprises 40 weight percent or less of the total weight of the bicomponent fiber.
11. A spunbonded nonwoven web comprising An elastomeric bicomponent fiber as claimed in any one of claims 1 to 10.
12. The spunbond nonwoven web of claim 11, wherein the nonwoven web is post-bonded.
13. The spunbond nonwoven web of claim 11 or 12, wherein the nonwoven web is apertured.
14. The spunbond nonwoven web of claim 11 or 12, wherein the nonwoven web exhibits a cup compression stiffness of 20 grams-force (gf) or less, or a normalized cup compression stiffness of 2.1 gf / gsm or less, based on a nonwoven web having a basis weight of 48 grams per square meter (gsm).
15. An elastomeric laminate comprising a spunbond nonwoven web facing and a backing, the spunbond nonwoven web comprising elastomeric bicomponent fibers, wherein the elastomeric bicomponent fibers include a core comprising a polypropylene-based elastomer and a secondary amide; and at least one sheath, the at least one sheath being free of secondary amides; wherein said at least one sheath constitutes less than 50 weight percent of the total weight of said bicomponent fiber; wherein the sheath comprises a polyethylene polymer, the secondary amide is present in the core in an amount of 0.1% to 10% by weight based on the weight of the core, and the secondary amide is a fatty acid amide.
16. The elastomeric laminate of claim 15, wherein the backing comprises an elastic film.
17. An absorbent article formed from the nonwoven web of claim 11 or the laminate of claim 15.
Citation Information
Patent Citations
Bed pad
US20040060112A1
Process for forming non-woven filamentary structures from fiber-forming synthetic organic polymers
US3338992A
Sheets of randomly distributed continuous filaments
US3341394A
Bonded nonwoven sheets with a defined distribution of bond strengths
US3502538A
Process of producing non-woven fabric fleece
US3502763A