Double-sided adhesive tape for electrolyte-resistant battery and preparation method thereof
By optimizing the mass ratio of the acrylic polymer and the additive combination, an adhesive layer with high initial adhesion and electrolyte resistance is formed, which solves the problem of easy corrosion of acrylic tape in a lithium battery environment and improves the adhesive performance and resistance of the tape. High temperature resistance.
Patent Information
- Application Number
- CN202211287216.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-20
AI Technical Summary
Existing acrylic pressure-sensitive tapes are prone to corrosion in the lithium battery environment, resulting in insufficient bonding performance and high temperature resistance. They cannot effectively fix the battery cells and battery packaging, leading to abnormal phenomena such as short circuits in the battery cells.
Using specific mass ratios of acrylic acid, lauryl methacrylate, glycidyl methacrylate, azobisisobutyronitrile and dibenzoyl peroxide, diglycidyl aniline and isophorone diisocyanate, and dioxide Materials such as silicon and KH570 organically modified silica form a polymer structure with high initial adhesion, peel strength and electrolyte resistance, enhancing the adhesion and heat resistance of the adhesive layer.
It significantly improves the initial adhesion, peel strength, electrolyte resistance and high temperature resistance of the tape, extends the service life of the tape, and maintains good bonding performance in the lithium battery environment.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of double-sided adhesive tapes, with an IPC classification number of C09J7 / 38, and in particular to a double-sided adhesive tape for an electrolyte-resistant battery and a preparation method thereof. Background Art
[0002] Pressure-sensitive tapes occupy an important position in adhesives, among which acrylic pressure-sensitive tapes are the most commonly used on the market, because this type of acrylic tape has great advantages in terms of cost, process, and performance, and has superior overall performance. These multiple advantages are unmatched by other types of tapes. With the continuous development of pure electric vehicles, smart phones, artificial intelligence machines, etc., and my country's strong support for new energy, the lithium battery industry has achieved unprecedented development. Therefore, it has also driven the development of industries related to lithium batteries. Double-sided tapes for batteries are used to bond the battery cells and the inner surface of the battery cell packaging to prevent the battery cells from shaking, causing abnormal phenomena such as battery cell short circuits, but conventional acrylic pressure-sensitive adhesives are not resistant to electrolytes, which will cause the double-sided tape to fall off and fail to fix and bond the battery cells and the inner surface of the battery cell packaging.
[0003] To solve the above problems, the application document with patent number CN202022039461 discloses an electrolyte-resistant tape. The electrolyte-resistant tape is provided with an anti-corrosion layer, which can prevent the battery electrolyte from corroding the tape and extend the service life of the tape. However, the bonding performance of the tape is not significantly improved.
[0004] The application document with patent number CN201811193151.8 discloses an electrolyte-resistant pressure-sensitive adhesive for tabs and a preparation method thereof, and an electrolyte-resistant tab tape. The raw materials of the tape include: acrylic monomer, initiator, ferric chloride, triphenyl phosphine, curing agent, and epoxidized polybutadiene. It solves the problem that the tape is easily carbonized and blackened, and solves the problem that small molecule oligomers are easily decomposed during the charging and discharging process. However, the high temperature resistance and bonding performance of the tape are not significantly improved. Summary of the invention
[0005] In order to solve the above problems, the first aspect of the present invention provides a double-sided adhesive tape for electrolyte-resistant batteries, which comprises a release film or a release paper, a base layer, and an adhesive layer.
[0006] Preferably, the adhesive layer is located on both sides of the base layer, and the release layers are located on the outside of the adhesive layer.
[0007] Preferably, the release film or release paper is a release film or release paper coated with a non-silicon release layer, the release film has a thickness of 25 μm-50 μm, the release paper has a thickness of 90-130 μm, and the release film or release paper is self-coated;
[0008] More preferably, the release film is a PET film with a thickness of 30 μm, purchased from Dongwan Zhonglian Electronic Materials Co., Ltd.; the release paper has a thickness of 110 μm, purchased from Dongguan Boya Adhesive Products Co., Ltd.
[0009] Further preferably, the non-silicon release layer raw material includes (by weight): 0.1-0.2 parts of release agent, 100-120 parts of diluent;
[0010] More preferably, the non-silicone release agent includes one or a mixture of two of PEELOIL1010, K100H, K100D, K100ES, and RL-600.
[0011] More preferably, the non-silicone release agent is PEELOIL1010.
[0012] More preferably, the PEELOIL1010 is purchased from Jiangshan Chemical (Shanghai) Co., Ltd.; the toluene (CAS No.: 108-88-3).
[0013] Preferably, the base layer includes one or more of PP film, PVC film, PET film, PI film, PE film, PTFE film, PC film, PO film, and PA film.
[0014] More preferably, the base layer film is a PET film.
[0015] More preferably, the thickness of the PET film is 20 to 30 μm.
[0016] More preferably, the thickness of the PET film is 30 μm.
[0017] More preferably, the PET film is purchased from Dongwan Zhonglian Electronic Materials Co., Ltd. Preferably, the thickness of the adhesive layer is 5 to 15 μm.
[0018] More preferably, the glue layer has a thickness of 10 μm.
[0019] Preferably, the raw materials of the adhesive layer include (by mass): 50-90 parts of acrylic monomer, 150-250 parts of solvent, 0.1-1 parts of initiator, 1-2 parts of curing agent, 0.4-1 parts of filler, 3-10 parts of tackifying resin, and 5-10 parts of color paste.
[0020] Preferably, the color paste includes one or more of phthalocyanine blue, cobalt green, and brilliant blue.
[0021] More preferably, the color paste is cobalt green (CAS No.: 19381-50-1), purchased from Laizhou Caizhiyuan Pigment Technology Co., Ltd.
[0022] Preferably, the solvent includes one or more of ethyl acetate, ethanol and toluene.
[0023] More preferably, the solvent is ethyl acetate, and ethyl acetate (CAS No.: 15604-36-1) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0024] Preferably, the acrylic monomer includes 1-3 parts of acrylic acid, 1-3 parts of hydroxypropyl acrylate, 1-10 parts of isobornyl acrylate, 1-5 parts of glycidyl methacrylate, 40-60 parts of isooctyl acrylate, and 5-10 parts of lauryl methacrylate.
[0025] Preferably, the mass ratio of acrylic acid, lauryl methacrylate and glycidyl methacrylate is (1-3):(4-5):(2-4).
[0026] More preferably, the mass ratio of acrylic acid, lauryl methacrylate and glycidyl methacrylate is 2:5:3.
[0027] The polymer used to prepare the adhesive layer needs a certain cross-linking density to ensure a certain cohesive strength, so that the adhesive layer can maintain its adhesion to the battery. The addition of acrylic acid can form a certain network structure in the polymer, which increases the cohesive strength of the polymer. However, as the amount of acrylic acid increases, the cross-linked network structure of the polymer increases, and the cohesive strength is too high, which will lead to a decrease in the wettability of the adhesive layer surface, and a decrease in the initial adhesion and peel strength of the adhesive layer to the PET substrate and the battery. The applicant found that when the mass ratio of acrylic acid, lauryl methacrylate and glycidyl methacrylate is (1-3): (4-5): (2-4), the adhesive layer has strong adhesion to the PET substrate and initial adhesion to the battery. The applicant speculates that acrylic acid, lauryl methacrylate and glycidyl methacrylate act synergistically during the polymerization process. In a certain polymer cross-linked network structure, the cohesive strength of the polymer is reduced, the creep of the molecular chain is enhanced, and the wettability to the substrate and the adhesion surface is enhanced, thereby improving the adhesion of the adhesive layer to the PET substrate and the initial adhesion to the battery. In addition, under the synergistic effect of the three, the network structure in the polymer can still enable it to have sufficient cohesive strength to cope with the strong corrosion of the electrolyte, thereby improving the electrolyte resistance of the tape.
[0028] Further preferably, the acrylic acid (CAS No.: 79-10-7) is purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; the lauryl methacrylate (CAS No.: 142-90-5) is purchased from Shanghai Hansi Chemical Co., Ltd.; and the glycidyl methacrylate (CAS No.: 106-91-2) is purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0029] Preferably, the initiator includes one or more of an azo initiator and a peroxide initiator.
[0030] More preferably, the azo initiator includes one or more of azobisisobutyronitrile and azobisisoheptylnitrile; and the peroxide initiator includes dibenzoyl peroxide.
[0031] More preferably, the initiator is azobisisobutyronitrile or benzoyl peroxide.
[0032] More preferably, the mass ratio of azobisisobutyronitrile to dibenzoyl peroxide is (1-3):(2-6).
[0033] More preferably, the mass ratio of azobisisobutyronitrile to dibenzoyl peroxide is 1:2.
[0034] Under the action of the initiator, each monomer undergoes a polymerization reaction to generate a polymer with a relatively large molecular weight. When the molecular weight is too large, the cohesive strength increases, the surface wettability decreases, and the peel strength and initial adhesion decrease. However, when the molecular weight is too small, the stability and electrolyte resistance of the adhesive layer are poor. The applicant has found that when the mass ratio of azobisisobutyronitrile and dibenzoyl peroxide is (1-3): (2-6), the wettability of the surface of the tape increases, and the initial adhesion and peel strength increase. The applicant speculates that the specific amount of azobisisobutyronitrile and dibenzoyl peroxide widens the molecular weight distribution of the synthesized molecules, increases the proportion of small molecular weight, increases the wettability of the surface of the tape, and improves the peel strength and initial adhesion of the adhesive layer without affecting the electrolyte resistance of the adhesive layer.
[0035] More preferably, the azobisisobutyronitrile (CAS No.: 78-67-1) is purchased from Jinan Huijinchuan Trading Co., Ltd.; the dibenzoyl peroxide (CAS No.: 94-36-0) is purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0036] Preferably, the curing agent includes one or more of isocyanate, epoxy, and amino curing agents.
[0037] Further preferably, the epoxy curing agent includes one or more of diglycidyl aniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, and resorcinol diglycidyl ether.
[0038] More preferably, the epoxy curing agent is diglycidyl aniline.
[0039] More preferably, the isocyanate curing agent includes one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate.
[0040] More preferably, the isocyanate curing agent is isophorone diisocyanate.
[0041] More preferably, the mass ratio of diglycidyl aniline, isophorone diisocyanate and isobornyl acrylate is 1:(3-5):(4-6).
[0042] More preferably, the mass ratio of diglycidyl aniline, isophorone diisocyanate and isobornyl acrylate is 1:4:5.
[0043] In order to ensure the adhesive layer's stickiness and electrolyte resistance, the cross-linked polymer molecules need to have a certain network structure to slow down the penetration of the electrolyte. Therefore, it is usually necessary to add a curing agent to increase the tight bonding between the polymer molecular chains. However, excessive use of curing agent will lead to a decrease in the initial adhesion and peel strength of the adhesive layer, affecting the normal use of the pressure-sensitive adhesive. The applicant found that when the mass ratio of diglycidyl aniline, isophorone diisocyanate and isobornyl acrylate is 1: (3-5): (4-6), the electrolyte resistance, heat resistance and bonding properties of the pressure-sensitive adhesive are improved. The applicant speculates that during the polymerization process, due to the high hardness and high glass transition temperature of isobornyl acrylate, it provides a certain heat resistance for the polymer. However, isobornyl acrylate will make the polymer more rigid in the early stage, cross-linking will occur to prevent chain growth, affect the internal structure of the copolymer, and reduce the electrolyte resistance. The steric hindrance of diglycidyl aniline is large, the contact angle is relatively large, and the electrolytic resistance is improved. Through the synergistic effect of the three, the initial cross-linking of isobornyl acrylate tends to react between molecular chains to form pseudo cross-linking, which will be restored after the curing agent completes its action, eliminating the impact on the internal structure of the copolymer and improving the bonding performance of the pressure-sensitive adhesive.
[0044] Further preferably, the diglycidyl aniline (CAS No.: 2095-06-9) was purchased from Hubei Zhenbo Chemical Co., Ltd.; the isophorone diisocyanate (CAS No.: 223-861-6) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; and the isobornyl acrylate (CAS No.: 5888-33-5) was purchased from Zhengzhou Alpha Chemical Co., Ltd.
[0045] Preferably, the filler includes one or more of silicon dioxide, carbon nanotubes, calcium sulfate whiskers, nanographite flakes, montmorillonite, kaolin, and talc.
[0046] More preferably, the filler is silica, KH570 organically modified silica.
[0047] More preferably, the average particle size of the silica is 20-40 nm, and the average particle size of the KH570 organic modified silica is 20-40 nm.
[0048] It is further preferred that the average particle size of the silica is 20 nm, and the average particle size of the KH570 organic modified silica is 20 nm.
[0049] More preferably, the weight ratio of the silica to the KH570 organic modified silica is 1:(10-15).
[0050] More preferably, the weight ratio of the silica to the KH570 organic modified silica is 1:12.
[0051] The poor electrolyte resistance of the pressure-sensitive adhesive may be due to the fact that the lithium-ion battery produces highly corrosive HF during the charging and discharging process. The invasion of HF into the adhesive layer will promote the decomposition of the polymer and cause the adhesive performance of the pressure-sensitive adhesive to decrease. In addition, the temperature of the battery will rise to a certain extent during use, which will affect the stability of the pressure-sensitive adhesive. Since silica reacts with HF and the product is a precipitate, it is speculated that when silica is added to the polymer to make a glue, HF is more likely to react with the substance that produces the precipitate, weakening the decomposition effect of HF on the polymer in the glue layer; and silica, as a rigid substance, can play the role of a skeleton and improve the heat resistance of the pressure-sensitive adhesive. However, the surface of silica is rich in hydrophilic groups and has poor dispersibility in the glue. KH570 organic modified silica is used to improve its compatibility. The applicant found that when the weight ratio of silica and KH570 organic modified silica is 1: (10-15), the prepared pressure-sensitive adhesive has good electrolyte resistance and heat resistance, especially above 100°C, and can maintain good performance.
[0052] More preferably, the silica, KH570 organic modified silica, is purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., and the model of KH570 organic modified silica is 100363.
[0053] Preferably, the tackifying resin includes one or more of rosin, rosin derivatives, and terpene resins.
[0054] More preferably, the thickening resin is a rosin derivative, and the rosin derivative includes one or more of hydrogenated rosin, disproportionated rosin, polymerized rosin, esterified rosin, and maleated rosin.
[0055] More preferably, the rosin derivatives are hydrogenated rosin and esterified rosin.
[0056] More preferably, the mass ratio of the rosin, esterified rosin and isooctyl acrylate is (1-2): (3-4): (10-20).
[0057] More preferably, the mass ratio of the rosin, esterified rosin and isooctyl acrylate is 1:4:15.
[0058] Adding tackifying resin can make the polymer form a certain network structure, but when the amount of tackifying resin is too large, it will cause entanglement between molecules, which will reduce the bonding performance of the pressure-sensitive adhesive. The applicant found that rosin, esterified rosin and isooctyl acrylate can work synergistically to improve the adhesion and stability of the pressure-sensitive adhesive. The applicant speculates that the tackifying resin makes the polymer form a network structure because the tackifying resin undergoes double bond copolymerization and esterification reactions during the polymerization process, but it also causes entanglement between molecules. When the three work together, the esterification reaction will be weakened without destroying the network structure, reducing the entanglement between molecules and improving the bonding performance of the pressure-sensitive adhesive.
[0059] Further preferably, the rosin (CAS No.: 8050-09-7), acid ester 150-170, was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; the esterified rosin was purchased from Shenzhen Vtolo Chemicals Co., Ltd, model FE-685; the isooctyl acrylate (CAS No.: 12080-30-9) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0060] More preferably, the hydroxypropyl acrylate (CAS No.: 25584-83-2) is purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0061] A second aspect of the present invention provides a method for preparing the electrolyte-resistant battery double-sided tape as described above, comprising the following steps:
[0062] (1) mixing 1-10 parts of isobornyl acrylate, 40-60 parts of isooctyl acrylate, 5-10 parts of lauryl methacrylate and 80-100 parts of a solvent, and stirring the mixture to obtain a mixed solution A;
[0063] Mix 1-3 parts of acrylic acid, 1-3 parts of hydroxypropyl acrylate, 1-5 parts of glycidyl methacrylate, 0.1-0.2 parts of initiator and 20-30 parts of solvent to obtain a mixed solution B;
[0064] Mix 0.2-0.4 parts of an initiator and 10-20 parts of a solvent to obtain a mixed solution C;
[0065] (2) Adding the mixed solution A into a reactor, controlling the stirring speed to 100-300 rpm, introducing an inert gas to expel the air, heating to 82-83° C. under reflux, dripping the mixed solution B into the reactor at a rate of 0.2 parts / min, and controlling the dripping to be completed within 2-2.5 hours, and continuing the reflux reaction for 1-1.5 hours;
[0066] (3) Slowly dropwise add half of the mixed solution C at a rate of 0.15 parts / min, and reflux at 80-81°C for 2 h after the dropwise addition;
[0067] (4) adding the remaining amount of the mixed solution C at a rate of 0.3 parts / min, and refluxing at 78-80°C for 2-2.5 hours after the addition is complete. After the reaction is complete, the temperature is lowered to below 40°C to obtain the electrolyte-resistant pressure-sensitive adhesive E.
[0068] (5) 80-120 parts of electrolyte resistant pressure sensitive adhesive E, 80-120 parts of solvent, a formulated amount of curing agent, tackifying resin, color paste, and filler are prepared into a glue coating liquid;
[0069] (6) preparing a release layer coating liquid by mixing a formulated amount of a release agent and a diluent, coating the release layer coating liquid on one side of a PET film having a thickness of 25-50 μm or a release paper having a thickness of 90-130 μm by a precision coating machine, and drying at a temperature of 90-120° C. to obtain a non-silicone release film or non-silicone release paper;
[0070] (7) applying a glue coating liquid on one side of the substrate by a precision coating machine, drying the substrate at a temperature gradient of 70-130° C. to obtain a glue layer, and then laminating the substrate with a non-silicon release film or non-silicon release paper to obtain a semi-finished product 1;
[0071] (8) Apply glue coating liquid on the release surface of the non-silicone release film or non-silicone release paper, dry it at a temperature gradient of 70-130° C. to obtain a glue layer, and then adhere it to the other side of the substrate of the semi-finished product 1 to obtain a double-sided tape product.
[0072] Beneficial Effects
[0073] 1. The initial adhesion, peel strength and electrolyte resistance of the tape are improved by controlling the mass ratio of acrylic acid, lauryl methacrylate and glycidyl methacrylate in acrylic monomers to (1-3): (4-5): (2-4).
[0074] 2. By controlling the mass ratio of azobisisobutyronitrile and dibenzoyl peroxide to (1-3): (2-6), the peel strength, initial adhesion and sustained adhesion of the pressure-sensitive adhesive can be effectively improved.
[0075] 3. By controlling the mass ratio of diglycidyl aniline, isophorone diisocyanate and isobornyl acrylate to 1:(3-5):(4-6), the electrolyte resistance, heat resistance and bonding performance of the pressure-sensitive adhesive are effectively improved.
[0076] 4. By controlling the weight ratio of silica and KH570 organic modified silica to 1:(10-15), the heat resistance and electrolyte resistance of the pressure sensitive adhesive are effectively improved.
[0077] 5. By controlling the mass ratio of rosin, esterified rosin and isooctyl acrylate to (1-2): (3-4): (10-20), the bonding performance and stability of the pressure-sensitive adhesive are effectively improved. Example
[0078] Example 1
[0079] Embodiment 1 provides a double-sided adhesive tape for electrolyte-resistant batteries, comprising a release film, a base layer, and an adhesive layer;
[0080] The adhesive layer is located on both sides of the base layer, and the release layers are located on the outside of the adhesive layer respectively;
[0081] The release film is a release film coated with a non-silicon release layer, the thickness of the release film is 30 μm, and the release film is self-coated; the raw materials of the non-silicon release layer are (by weight): 0.1 parts of release agent and 100 parts of diluent; the release film is a PET film, purchased from Dongwan Zhonglian Electronic Materials Co., Ltd.; the release agent is PEELOIL1010, purchased from Jiangshan Chemical (Shanghai) Co., Ltd., and the diluent is toluene (CAS No.: 108-88-3).
[0082] The substrate layer is a PET film with a thickness of 30 μm, purchased from Dongwan Zhonglian Electronic Materials Co., Ltd.
[0083] The thickness of the adhesive layer is 10 μm.
[0084] The raw materials of the adhesive layer include (by mass): 71.5 parts of acrylic monomer, 0.5 parts of initiator, 1.5 parts of curing agent, 0.5 parts of filler, 10 parts of tackifying resin, 220 parts of solvent, and 5 parts of color paste.
[0085] The color paste is cobalt green (CAS No.: 19381-50-1), purchased from Laizhou Caizhiyuan Pigment Technology Co., Ltd.
[0086] The solvent is ethyl acetate, and ethyl acetate (CAS No.: 15604-36-1) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0087] The acrylic monomers of the raw materials of the adhesive layer include (by mass): 2 parts of acrylic acid, 3 parts of hydroxypropyl acrylate, 8.5 parts of isobornyl acrylate, 3 parts of glycidyl methacrylate, 50 parts of isooctyl acrylate, and 5 parts of lauryl methacrylate.
[0088] The mass ratio of acrylic acid, lauryl methacrylate and glycidyl methacrylate is 2:5:3.
[0089] The acrylic acid (CAS No.: 79-10-7) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; the lauryl methacrylate (CAS No.: 142-90-5) was purchased from Shanghai Hansi Chemical Co., Ltd.; and the glycidyl methacrylate (CAS No.: 106-91-2) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0090] The initiators are azobisisobutyronitrile and dibenzoyl peroxide, and the mass ratio of azobisisobutyronitrile to benzoyl peroxide is 1:2.
[0091] The azobisisobutyronitrile (CAS No.: 78-67-1) was purchased from Jinan Huijinchuan Trading Co., Ltd.; the dibenzoyl peroxide (CAS No.: 94-36-0) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0092] The curing agent is diglycidyl aniline and isophorone diisocyanate, and the mass ratio of diglycidyl aniline, isophorone diisocyanate and isobornyl acrylate is 1:4:5.
[0093] The diglycidyl aniline (CAS No.: 2095-06-9) was purchased from Hubei Zhenbo Chemical Co., Ltd.; the isophorone diisocyanate (CAS No.: 223-861-6) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; the isobornyl acrylate (CAS No.: 5888-33-5) was purchased from Zhengzhou Alpha Chemical Co., Ltd.
[0094] The filler is silicon dioxide, KH570 organic modified silicon dioxide; the average particle size of silicon dioxide is 20nm, the average particle size of KH570 organic modified silicon dioxide is 20nm; the weight ratio of silicon dioxide to KH570 organic modified silicon dioxide is 1:12.
[0095] The silica, KH570 organic modified silica, was purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., and the model of KH570 organic modified silica is 100363.
[0096] The tackifying resin is rosin, esterified rosin; the mass ratio of rosin, esterified rosin and isooctyl acrylate is 1:4:15.
[0097] The rosin (CAS No.: 8050-09-7), acid ester 150-170, was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; the esterified rosin was purchased from Shenzhen Vtolo Chemicals Co., Ltd., model FE-685; the isooctyl acrylate (CAS No.: 12080-30-9) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0098] The hydroxypropyl acrylate (CAS No.: 25584-83-2) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0099] A method for preparing the electrolyte-resistant battery double-sided tape as described above comprises the following steps:
[0100] (1) 8.5 parts of isobornyl acrylate, 50 parts of isooctyl acrylate, 5 parts of lauryl methacrylate and 80 parts of a solvent were mixed and stirred to obtain a mixed solution A;
[0101] Mix 2 parts of acrylic acid, 3 parts of hydroxypropyl acrylate, 3 parts of glycidyl methacrylate, 0.1 parts of initiator and 20 parts of solvent to obtain a mixed solution B;
[0102] Mix 0.4 parts of the initiator and 20 parts of the solvent to obtain a mixed solution C;
[0103] (2) Add the mixed solution A into the reactor, control the stirring speed to 200 rpm, introduce inert gas to expel the air, raise the temperature to 83°C and under reflux, drip the mixed solution B into the reactor at a rate of 0.2 parts / min, and control the dripping to be completed within 2.5 hours, and continue the reflux reaction for 1.5 hours;
[0104] (3) Slowly add half of the mixed solution C at a rate of 0.15 parts / min, and reflux at 81°C for 2 h after the addition is complete;
[0105] (4) adding the remaining amount of the mixed solution C dropwise at a rate of 0.3 parts / min, and refluxing at 80° C. for 2.5 hours after the addition is complete. After the reaction is complete, the temperature is lowered to below 40° C. to obtain E;
[0106] (5) 100 parts of electrolyte resistant pressure sensitive adhesive E are added with 100 parts of solvent, a formulated amount of curing agent, color paste, and filler to prepare a glue coating liquid;
[0107] (6) preparing a release layer coating liquid by mixing a formulated amount of release agent and a diluent, coating the release layer coating liquid on one side of the PET film by a precision coating machine, and drying at a temperature of 100° C. to obtain a non-silicone release film;
[0108] (7) applying a glue coating liquid on one side of the substrate by a precision coating machine, drying the adhesive layer by gradient drying at 100° C., 110° C., 70° C., 90° C., 120° C., 130° C., 110° C., 90° C., and 80° C., and then laminating a non-silicone release film to obtain a semi-finished product 1;
[0109] (8) Apply glue coating liquid on the release surface of the non-silicone release film, and dry it at 100° C., 110° C., 70° C., 90° C., 120° C., 130° C., 110° C., 90° C., and 80° C. to obtain a glue layer, and then adhere it to the other side of the substrate of the semi-finished product 1 to obtain a double-sided tape product.
[0110] Example 2
[0111] The difference from Example 1 is that the mass ratio of diglycidyl aniline, isophorone diisocyanate and isobornyl acrylate is 1:5:2.
[0112] Example 3
[0113] The difference from Example 1 is that the mass ratio of the rosin, esterified rosin and isooctyl acrylate is 2:4:15.
[0114] Comparative Example 1
[0115] The difference from Example 1 is that the acrylic acid monomer is 3 parts of hydroxypropyl acrylate, 5 parts of isobornyl acrylate, 3 parts of glycidyl methacrylate, 50 parts of isooctyl acrylate, and 5 parts of lauryl methacrylate.
[0116] Comparative Example 2
[0117] The difference from Example 1 is that the initiator is dibenzoyl peroxide.
[0118] Comparative Example 3
[0119] The difference from Example 1 is that the curing agent is isophorone diisocyanate.
[0120] Comparative Example 4
[0121] The difference from Example 1 is that the filler is talcum powder.
[0122] The talc powder was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0123] Comparative Example 5
[0124] The difference from Example 1 is that the esterified rosin is replaced by hydrogenated rosin.
[0125] The hydrogenated rosin (CAS No.: 1446-61-3) was purchased from (Alpha) Henan Weitixi Chemical Technology Co., Ltd.
[0126] Performance Testing
[0127] 1. Adhesion
[0128] (1) Initial viscosity
[0129] The initial tackiness of the electrolyte-resistant double-sided adhesive tapes obtained in Examples 1-3 and Comparative Examples 1-5 was tested in accordance with GB / T4852-84 Initial tackiness of pressure-sensitive adhesive tapes. The results are recorded in Table 1.
[0130] (2) 180° peel strength
[0131] The electrolyte-resistant double-sided adhesive tapes for batteries obtained in Examples 1-3 and Comparative Examples 1-5 were tested for 180° peel strength. The test method was in accordance with GB / T 2792-2014 180° peel strength test for pressure-sensitive adhesive tapes, and the results were recorded in Table 1.
[0132] (3) Maintaining viscosity
[0133] The electrolyte-resistant double-sided adhesive tapes for batteries obtained in Examples 1-3 and Comparative Examples 1-5 were tested for their stickiness. The test method was in accordance with GB / T4851-2014 for determination of stickiness of pressure-sensitive adhesive tapes, and the results were recorded in Table 1.
[0134] 2. Electrolyte resistance
[0135] The electrolyte resistance performance of the electrolyte-resistant battery double-sided adhesive tape obtained in Examples 1-3 and Comparative Examples 1-5 was tested. Two battery separators were bonded together with double-sided adhesive tape, and then immersed in an electrolyte at 85°C for 24 hours. The tape did not change color, fall off, or bulge. The results are recorded in Table 1.
[0136] The electrolyte was purchased from Nanjing Mojies Energy Technology Co., Ltd., product number 10045517054728.
[0137] 3. High temperature resistance
[0138] The high temperature resistance performance of the electrolyte resistant battery double-sided tape obtained in Examples 1-3 and Comparative Examples 1-5 was tested. The high temperature resistance performance was that the tape had no shrinkage deformation and no residual adhesive when flatly attached to a steel plate and heated at 130°C for 1 hour. The results are recorded in Table 1.
[0139] Note:
[0140] 1. Adhesion
[0141] (1) Initial adhesion (#) is denoted by Q: Q ≥ 12 is excellent; 9 ≤ Q < 12 is good; 6 ≤ Q < 9 is qualified; Q < 6 is unqualified.
[0142] (2) 180° peel strength (N / 25cm) is denoted as σ 180°:σ 180° ≥9 is excellent; 7≤σ 180° <9 is good; 5≤σ 180° <7 is qualified; σ 180° <5 means unqualified.
[0143] (3) The stickiness (h) is denoted as t: t ≥ 30 is excellent; 25 ≤ t < 30 is good; 15 ≤ t < 25 is qualified; t < 15 is unqualified.
[0144] 2. Electrolyte resistance
[0145] Ten parallel samples of Examples 1-3 and Comparative Examples 1-5 were respectively set to test the electrolyte resistance performance. The number of samples with delamination, falling and fading was recorded as n, where n≤2 was excellent; 2<n≤4 was good; 4<n≤6 was qualified; and n>6 was unqualified.
[0146] 3. High temperature resistance
[0147] The percentage of the residual glue area on the test steel plate to the area of the steel plate is recorded as S, S≤5% is excellent, 5%<S ≤10% is good; 10%<S≤20% is qualified; S>20% is unqualified.
[0148] Table 1
[0149]
Claims
1. A double-sided adhesive tape for electrolyte-resistant batteries, characterized in that: The composition includes one of a release film or a release paper, a base layer, and a glue layer; The adhesive layer is located on both sides of the base layer, and the release layers are located on the outside of the adhesive layer respectively; The release film or release paper is a release film or release paper coated with a non-silicon release layer, the thickness of the release film is 25 μm-50 μm, the thickness of the release paper is 90-130 μm, and the release film or release paper is self-coated; The non-silicon release layer raw materials include: by weight, 0.1-0.2 parts of release agent, 100-120 parts of diluent; The substrate layer comprises a PET film; The adhesive layer raw materials, by weight: 50-90 parts of acrylic monomer, 0.1-1 parts of initiator, 3-10 parts of curing agent, 0.4-1 parts of filler, 5-10 parts of tackifying resin, 150-250 parts of solvent, 5-10 parts of color paste; The acrylic acid monomer comprises 1-3 parts of acrylic acid, 1-3 parts of hydroxypropyl acrylate, 1-10 parts of isobornyl acrylate, 1-5 parts of glycidyl methacrylate, 40-60 parts of isooctyl acrylate, and 5-10 parts of lauryl methacrylate; the mass ratio of acrylic acid, hydroxypropyl acrylate, and glycidyl methacrylate is (1-3): (4-5): (2-4); The initiator is azobisisobutyronitrile and dibenzoyl peroxide, and the mass ratio of azobisisobutyronitrile to dibenzoyl peroxide is (1-3): (2-6); The curing agent includes one or more of an isocyanate curing agent, an epoxy curing agent, and an amino curing agent; The isocyanate curing agent is isophorone diisocyanate, the epoxy curing agent is diglycidyl aniline, and the mass ratio of diglycidyl aniline, isophorone diisocyanate and isobornyl acrylate is 1:(3-5):(4-6); The filler is silicon dioxide, KH570 organic modified silicon dioxide; The average particle size of the silicon dioxide is 20-40 nm, and the average particle size of the KH570 organic modified silicon dioxide is 20-40 nm; The weight ratio of the silica to KH570 organic modified silica is 1:(10-15); The tackifying resin is a rosin derivative; The rosin derivatives are rosin and esterified rosin; The mass ratio of the rosin, esterified rosin and isooctyl acrylate is (1-2): (3-4): (10-20).
2. A method for preparing a double-sided adhesive tape for an electrolyte-resistant battery according to claim 1, characterized in that: The method for preparing the double-sided adhesive tape for electrolyte-resistant batteries comprises the following steps: (1) Mix 1-10 parts of isobornyl acrylate, 40-60 parts of isooctyl acrylate, 5-10 parts of lauryl methacrylate and 80-100 parts of solvent, and stir evenly to obtain a mixed solution A; Mix 1-3 parts of acrylic acid, 1-3 parts of hydroxypropyl acrylate, 1-5 parts of glycidyl methacrylate, 0.1-0.2 parts of initiator and 20-30 parts of solvent to obtain a mixed solution B; Mix 0.2-0.4 parts of an initiator and 10-20 parts of a solvent to obtain a mixed solution C; (2) Add the mixed solution A into the reactor, control the stirring speed to 100-300 rpm, introduce inert gas to expel the air, raise the temperature to 82-83°C and reflux, then drip the mixed solution B into the reactor at a rate of 0.2 parts / min. After the dripping is completed within 2-2.5 hours, continue the reflux reaction for 1-1.5 hours; (3) Slowly add half of the mixed solution C at a rate of 0.15 parts / min. After the addition is complete, reflux at 80-81°C for 2 hours. (4) adding the remaining amount of the mixed solution C dropwise at a rate of 0.3 parts / min, and refluxing at 78-80°C for 2-2.5 hours after the addition is complete. After the reaction is complete, cooling to below 40°C and discharging the material to obtain an electrolytic pressure-sensitive adhesive E; (5) 80-120 parts of electrolyte resistant pressure sensitive adhesive E, 80-120 parts of solvent, a formulated amount of curing agent, tackifying resin, color paste, and filler are prepared into a glue coating liquid; (6) preparing a release layer coating liquid by mixing a formulated amount of release agent and a diluent, coating the release layer coating liquid on one side of a PET film with a thickness of 25-50 μm or a release paper with a thickness of 90-130 μm by a precision coating machine, and drying at a temperature of 90-120° C. to obtain a non-silicone release film or non-silicone release paper; (7) coating a glue coating liquid on one side of the substrate with a precision coating machine, drying the glue layer with a temperature gradient of 70-130° C., and then laminating a non-silicon release film or non-silicon release paper to obtain a semi-finished product 1; (8) Applying glue coating liquid on the release surface of the non-silicone release film or non-silicone release paper, drying with a temperature gradient of 70-130° C. to obtain a glue layer, and then laminating the other side of the substrate of the semi-finished product 1 to obtain a double-sided tape product.