A method for preparing a synergistically enhanced light-controlled humidity-regulating fiber membrane

By copolymerizing acryloyl spiropyran with co-regulators and using electrospinning technology to prepare nanofiber materials, the active adjustment of humidity is achieved by alternating UV-visible light irradiation, which solves the problems of single function and limited adjustment ability of existing materials. , improving the efficiency and adaptability of humidity regulation.

CN115821486BActive Publication Date: 2024-10-11INNER MONGOLIA NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211106514.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-12
Publication Date
2024-10-11
Estimated Expiration
2042-09-12

AI Technical Summary

Technical Problem

Existing humidity control materials have a single function and are unable to actively adjust humidity according to the external environment. They also rely only on spiropyran molecules to regulate their limited ability and cannot meet the needs of modern life.

Method used

By copolymerizing acryloyl spiropyran with co-regulators acrylic acid and methyl methacrylate, and using electrospinning technology to prepare porous water-permeable nanofiber materials, the humidity can be adjusted through alternating UV-visible light irradiation.

Benefits of technology

It achieves controllable humidity adjustment, enhances the adjustment ability of the material, can actively adjust according to the external environmental humidity, adapts to complex environmental conditions, and improves life and health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115821486B_ABST
    Figure CN115821486B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a synergistically enhanced light-controlled humidity-regulating fiber membrane, which utilizes acryloyl spiropyran to copolymerize with co-regulators acrylic acid and methyl methacrylate, and prepares a porous water-permeable nanofiber material by electrostatic spinning technology. The material is alternately irradiated with ultraviolet-visible light in a certain confined space. When the material is irradiated with ultraviolet light, the spiropyran molecules on the surface of the material open the ring to form oxygen anions and absorb water in coordination with acrylic acid, and the humidity in the space is reduced at this time; when the material is irradiated with visible light, the spiropyran molecules on the surface of the material restore the closed-loop hydrophobic state, and the material releases water molecules at this time, causing the humidity in the space to rise. The purpose of regulating the humidity in a confined space can be achieved by alternating irradiation of controllable ultraviolet-visible light, providing a certain theoretical basis for solving the problem of regulating the humidity of indoor air. The addition of acrylic acid makes the spiropyran polymer molecules more stable, and the water absorption effect is significantly improved compared with that without adding acrylic acid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic functional materials, and mainly relates to a light-controlled humidity-regulating nanofiber membrane with a synergistic enhancement effect and a preparation method thereof. Background Art

[0002] A dry indoor environment can make people feel tight skin and sore throats, and it can also increase the amount of suspended dust in the air, greatly increasing the chances of virus particles invading the human body, and even speeding up the spread of various infectious diseases. Therefore, appropriate indoor air humidity is very important for people's normal health. This patent aims to develop a light-controlled intelligent humidity-regulating material that can greatly save the cost of organic raw materials.

[0003] At present, there have been a large number of research and scientific research results on humidity control materials at home and abroad, but most of the existing products have a single function, that is, they can only absorb or release water in one direction, have poor adaptability, and cannot actively and reversibly adjust the ambient humidity according to the actual situation of the external environment. And there are few reports on the development of smart materials that use external stimuli to control the absorption and release of moisture. In recent years, smart control materials have attracted more and more attention due to their wide application in life. Compared with inorganic photosensitive materials, organic molecules have great advantages in chemical modification ability and reaction diversity. These photosensitive organic molecules usually undergo reversible transformation between two conformations under irradiation of light of different wavelengths. During the light-induced transformation, many physical and chemical properties of the surface change, such as surface free energy, absorption spectrum, dielectric constant, redox potential and geometric structure, etc. Organic molecular humidity control material products have strong shape plasticity, large moisture capacity, wide range of use, and great room for development. At present, the research on photochromic compounds is mostly focused on Shiff bases, azo compounds, fulgide, diarylethenes, spiropyrans, spirooxazines and related heterocyclic compounds, among which spiropyran compounds are the most representative.

[0004] Spiropyran is a SP 3 The two mutually perpendicular aromatic ring structures connected by the hybridized spiro carbon atoms have only a local conjugated structure, forming a closed-ring spiropyran (usually represented by SP). Its absorption spectrum is in the ultraviolet region. After being stimulated by appropriate external stimuli, the spiro oxygen bond in the molecule undergoes heterolytic cleavage and the two parts of the molecule rotate to become a metastable merocyanine structure (usually represented by MC) with two aromatic rings coplanar. The absorption wavelength moves to the visible light region and becomes a chromophore. The entire molecule forms a large conjugated system with a good conjugated structure. The oxygen anion formed by heterolytic cleavage of the CO bond will react with H +, amino acids, water, etc. to form coordination bonds or hydrogen bonds. The system can be closed again under visible light irradiation or heating conditions to form a colorless spiro ring structure. Therefore, spiropyran compounds have also been frequently used in the surface functionalization of materials in recent years. This type of photosensitive organic compound has the characteristics of high sensitivity, sensitivity to ultraviolet light and fast electron transfer speed.

[0005] In recent years, many studies have been conducted on the use of spiropyran compounds to prepare light-controlled wettability materials. However, these methods and techniques have many steps, complex preparation techniques, and are not conducive to large-scale preparation, making them difficult to meet practical applications. Electrospinning technology, as an effective method for preparing materials with controllable surface roughness and morphology, can solve the above problems. Electrospinning technology is simple, easy to operate, and low-cost, suitable for large-area material production. In addition, the electrospinning method can easily prepare porous and water-permeable fiber membranes, providing sufficient water storage space and providing basic conditions for effectively regulating humidity. Through continuous optimization of materials, it was found that the ability to regulate humidity only by materials containing spiropyran is limited and cannot meet the urgent application needs of modern production and life. Therefore, during the synthesis process, the original spiropyran molecule is combined with a co-regulator to achieve the requirement of synergistically enhancing the regulation ability.

[0006] In general, there are two problems in the field of humidity control: 1. There is a lack of new intelligent materials that can actively adjust humidity according to external humidity environment through external stimulation. Therefore, in order to improve people's living and health standards, it is necessary to develop an energy-saving, efficient, durable, simple and practical light-controlled humidity-regulating film. 2. Through research, it was found that the ability to regulate humidity by relying solely on spiropyran molecules is limited, so combining spiropyran with a co-regulator can greatly improve the material's ability to regulate humidity. Summary of the invention

[0007] The present invention intends to utilize acryloyl spiropyran to copolymerize with auxiliary regulators acrylic acid and methyl methacrylate, and prepare porous and water-permeable nanofiber materials through electrostatic spinning technology.

[0008] In a certain confined space, the material is alternately irradiated with ultraviolet and visible light. When the material is irradiated with ultraviolet light, the spiropyran molecules on the surface of the material open to form oxygen anions and absorb water in coordination with acrylic acid, and the humidity in the space decreases; when the material is irradiated with visible light, the spiropyran molecules on the surface of the material return to a closed-loop hydrophobic state, and the material releases water molecules, causing the humidity in the space to rise. The purpose of regulating the humidity in a confined space can be achieved through controllable alternating irradiation of ultraviolet and visible light, providing a certain theoretical basis for solving the problem of regulating indoor air humidity.

[0009] Since acrylic acid itself can form hydrogen bonds with water molecules, if the content of acrylic acid is too high, water molecules will form double hydrogen bonds with acrylic acid and cannot form hydrogen bonds with spiropyran, resulting in the material being unable to regulate humidity. Therefore, by changing the polymerization ratio of methyl methacrylate to acrylic acid to adjust the content of acrylic acid, the ability of the spiropyran molecular unit to regulate humidity can be effectively improved. A humidity regulating material with controllable regulating ability and the strongest synergistic effect was prepared, which solved the problems that existing products can only be passively regulated and have limited regulating ability.

[0010] To achieve the above-mentioned purpose, the present invention provides a method for preparing a fiber membrane that synergistically enhances the light-controlled humidity regulation capability, and the specific contents are as follows:

[0011] The present invention designs a method for preparing a fiber membrane with synergistically enhanced light-controlled humidity regulation capability, and the main technical scheme includes: the first step is to synthesize spiropyran monomer molecules, dissolve 2,3,3-trimethyl-3H-indole and 2-bromoethanol in anhydrous CH3CN (2,3,3-trimethyl-3H-indole:2-bromoethanol=1:1-1:1.5, n:n) to form a red solution. The red solution is refluxed and stirred under a nitrogen atmosphere until it is cooled to room temperature; the solvent anhydrous CH3CN is evaporated in vacuum to obtain a crude product. The crude product is recrystallized with acetone and washed with acetone to obtain compound 1, which is a light pink solid compound 1. Compound 1 and 5-nitrosalicylicylaldehyde are dissolved in anhydrous ethanol (compound 1:5-nitrosalicylicylaldehyde=1:1-1:1.2, n:n), heated to reflux, diethylamine is added and the mixture is refluxed under nitrogen, cooled to room temperature, and the anhydrous ethanol is removed in vacuum to obtain a solid. The obtained solid was washed with distilled water, and then chromatographed on a silica gel column using a mixture of ethyl acetate / petroleum ether (1 / 5, v / v) as an eluent to produce compound 2 SP-OH, which is a purple needle-shaped product. SP-OH and anhydrous dichloromethane were added to a round-bottom flask, and the solution was stirred at 0-5°C to completely dissolve SP-OH, and then acryloyl chloride was added dropwise to the mixed solution of SP-OH and anhydrous dichloromethane under a nitrogen atmosphere, and triethylamine was added dropwise while stirring continuously to form a mixture (SPOH: acryloyl chloride: triethylamine = 1:1:1-1:1.5:1.5, n:n:n), the mixture was refluxed at low heat and the solvent was removed using a rotary evaporator, and the obtained solid was washed with dichloromethane and extracted multiple times. The solid was chromatographed on a silica column using a mixture of ethyl acetate / petroleum ether (1 / 5, v / v) as an eluent to obtain a pale yellow solid spiropyran monomer molecule SPA.

[0012] Step 2: The spiropyran monomer SPA obtained in the first step is copolymerized with acrylic acid (AA) and methyl methacrylate (MMA) using AIBN as a thermal initiator to prepare a spiropyran copolymer. In a three-necked flask, SPA is dissolved in DMF under a nitrogen atmosphere. The temperature is controlled at 65-70°C, and a mixed solution of AA and MMA in a certain proportion (SPA:AA:MMA=1:0:10-1:4:6, n:n:n) is added. The specific feed ratio is shown in Table 1. Under constant magnetic stirring, AIBN is added and the solution is heated to 65-70°C. The polymerization is carried out under a nitrogen atmosphere for 24 hours. After cooling to room temperature, the copolymer is precipitated in distilled water 3 times to remove unreacted monomers and residual initiators, and the product is obtained. The product is vacuum dried at 30°C for 12 hours to obtain a spiropyran copolymer.

[0013] Step 3: Spiropyran polymers with different AA and MMA ratios were prepared into a DMF solution with a concentration of 45 wt%. The ambient temperature and relative humidity of the electrospinning process were maintained at 24 ± 1 °C and 20 ± 2%, respectively. The electrospinning needle was connected to a high-voltage power supply and a stable voltage of 16 kV was applied. Finally, the electrospun film was dried under vacuum at 30 °C to prepare a humidity-adjustable membrane material.

[0014] The fourth step is to test the water absorption and hydrophobicity process of the reversible humidity regulating material: first, the humidity regulating membrane material to be tested is irradiated with visible light to make the spiropyran molecules on the surface of the membrane material in a closed-loop state. At this time, the contact angle of the membrane material surface is 0.0447 W / m2. The membrane material is then irradiated with a 365nm ultraviolet lamp to open the ring of the spiropyran molecules on the surface of the membrane material and transform them all into hydrophilic partially indigo structures. At this time, the contact angle of the membrane material surface is tested again and it is found that the contact angle becomes smaller, indicating that the hydrophilicity of the membrane material surface is enhanced by ultraviolet light irradiation; at this time, the membrane material is irradiated with visible light again to transform the partially indigo molecules on the surface into hydrophobic spiropyran molecules. At this time, the contact angle of the membrane material surface is tested and it is found that the membrane material restores the original contact angle value, indicating that ultraviolet-visible light plays an important role in reversibly regulating the water absorption and hydrophobicity of the material.

[0015] The fifth step is to test the material's ability to reversibly regulate humidity: a glass container is used to simulate a microenvironment for regulating humidity. Before the test, a film cut into a certain volume (film area / space volume = 0.1 m 2 / m 3 ) is sealed in a glass container and left to stand until the temperature and humidity in the sealed container are constant. Then, an ultraviolet lamp and a visible light lamp are placed outside the glass container. When the film is irradiated with ultraviolet light, the humidity in the sealed glass container decreases until the humidity value remains constant. When the film is irradiated with visible light, the humidity value in the glass container increases.

[0016] In the second step, the molar ratios of SPA:AA:MMA are 1:0:10, 1:1:9, 1:2:8, 1:3:7 and 1:4:6, respectively.

[0017] Table 1 Molar ratio of spiropyran monomer, acrylic acid and methyl methacrylate in the embodiment

[0018] sample SPA AA MMA 1 1 0 10 2 1 1 9 3 1 2 8 4 1 3 7 5 1 4 6

[0019] At present, the development of traditional humidity control materials is mostly concentrated on porous inorganic materials such as charcoal, diatomaceous earth and zeolite. When the ambient humidity is high, water molecules are absorbed through their porosity, and when the ambient humidity is low, the water molecules in the pores are passively released. In addition, inorganic materials have great limitations in chemical modification and reaction diversity. More importantly, the humidity control materials currently studied can only passively adjust the humidity. Only when the ambient humidity reaches the extreme value (moisture absorption: RH = 70%, moisture release: RH = 50%) can the humidity respond. It cannot actively control and adjust the ambient humidity, making it impossible to adapt to complex and diverse environmental conditions, greatly limiting the application range of the product. The present invention can realize intelligent two-way humidity control through external stimuli (light, electricity, etc.). Moreover, by comparing Example 1 (without acrylic acid) with Examples 2-5 (with acrylic acid), it can be found that by creatively introducing acrylic acid (AA) into the copolymer block, the humidity adjustment range of the material is increased, solving the problem of limited adjustment range of existing spiropyran-based humidity control materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the reaction diagram of acrylic acid and spiropyran; a is the enthalpy change diagram, and b is the water absorption effect diagram.

[0021] Figure 2 Schematic diagram of the chemical reaction for preparing fiber membrane. DETAILED DESCRIPTION

[0022] The technical solutions in the present invention are described clearly and completely with examples below. Obviously, the present invention is not limited to the following examples. The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified. Based on the examples in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Because the carboxyl group in acrylic acid can cooperate with the oxygen anion of spiropyran ring opening to form a double hydrogen bond with a water molecule to improve the water absorption effect (see Figure 1 The reactants and products were calculated using the GAUSSIAN09 package. The geometry of the stationary points was optimized using the hybrid density functional m062x method. The enthalpy of formation data are an excellent way to determine whether theoretical predictions are likely to be stable, and these data can be used as a guide to evaluate possible reaction routes. The calculations found (see Figure 1a), when there is no carboxyl group, the enthalpy change of the water absorption process of the spiropyran polymer is -9.5 kcal / mol. When acrylic acid is added, the energy of the spiropyran polymer molecules is greatly reduced, indicating that the addition of acrylic acid makes the spiropyran polymer molecules more stable, and the enthalpy change of water absorption is -19.6 kcal / mol, which is significantly improved compared with the water absorption effect without adding acrylic acid.

[0024] A method for preparing a fiber membrane with synergistically enhanced light-controlled humidity regulation capability, the specific contents of which are as follows:

[0025] Figure 2 The present invention designs a method for preparing a fiber membrane with synergistically enhanced light-controlled humidity regulation capability. The main technical scheme includes: the first step is to synthesize spiropyran monomer molecules. The specific synthesis steps are as follows: Figure 2 As shown. 2,3,3-Trimethyl-3H-indole (3.18 g, 20.0 mmol) and 2-bromoethanol (2.48 g, 20.0 mmol) were dissolved in anhydrous CH3CN (30 mL). The red solution was refluxed under a nitrogen atmosphere for 12 hours while stirring continuously. After cooling to room temperature, the solvent (CH3CN) was evaporated in vacuo. The crude product was recrystallized from acetone and washed with acetone to give compound 1 as a light pink solid (compound 1). Next, compound 1 (4.54 g, 16.0 mmol) and 5-nitrosalicylicylaldehyde (2.67 g 16.0 mmol) were dissolved in anhydrous ethanol (40 mL). After heating to reflux, diethylamine (in 5 mL of anhydrous ethanol) was added and the mixture was refluxed under nitrogen for 5 hours. After cooling to room temperature, the solvent (ethanol) was removed in vacuo. The obtained solid was washed 3 times with distilled water, and then chromatographed on a silica gel column using a mixture of ethyl acetate / petroleum ether (1 / 5, v / v) as an eluent. The process produces compound 2 (SP-OH) as a purple needle-shaped product. SP-OH (3.52g, 10.0mmol) and 25mL of anhydrous dichloromethane were added to a 100mL round-bottom flask, and the solution was stirred under ice-cold conditions to completely dissolve SP-OH, and then 1.09g (12.0mmol) was added dropwise to the mixture under a nitrogen atmosphere to obtain acryloyl chloride. After continuous stirring for 30 minutes, triethylamine was added dropwise. The mixture was refluxed for 3 hours. The solvent was removed in vacuo, and the obtained solid was washed with dichloromethane and extracted 3 times. The crude product was chromatographed on a silica column using a mixture of ethyl acetate / petroleum ether (1 / 5, v / v) as an eluent. A pale yellow solid spiropyran monomer molecule (SPA) was obtained.

[0026] Step 2: SPA, AA and MMA were copolymerized with AIBN as thermal initiator to prepare spiropyran copolymer. In a 100 mL three-necked flask, 2.03 g (5.0 mmol) of SPA was dissolved in DMF (30 mL) under nitrogen atmosphere. The temperature was controlled at 65-70 ° C, and a certain proportion of a mixed solution of AA and MMA was added (the molar ratios of SPA:AA:MMA were 1:0:10, 1:1:9, 1:2:8, 1:3:7 and 1:4:6, respectively). Under constant magnetic stirring, 0.50 g of AIBN was added and the solution was heated to 65-70 ° C. The polymerization was carried out under nitrogen atmosphere for 24 hours. After cooling to room temperature, the copolymer was precipitated in 100 mL of distilled water 3 times to remove unreacted monomers and residual initiator. The product was vacuum dried at 30 ° C for 12 hours to obtain a spiropyran copolymer.

[0027] Step 3: Spiropyran polymers with different ratios of AA and MMA were prepared into a DMF solution with a concentration of 45wt%. Before electrospinning, the mixed solution was vigorously stirred at 30°C for 24 hours. The ambient temperature and relative humidity of the electrospinning process were maintained at 24±1°C and 20±2%, respectively. The electrospinning needle was connected to a high-voltage power supply and a stable voltage of 16kV was applied. The distance between the needle tip and the negatively charged roller collector was 18cm. The feed rate of the precursor solution was 1.0mL / h, which was controlled by a syringe pump. The spinning process of each film lasted for 3 hours. Finally, the electrospun film was dried under vacuum at 30°C to prepare a humidity-adjustable membrane material.

[0028] Step 4: Wettability is an important property for studying the water absorption of the material surface. The water absorption capacity of the material surface can be obtained by testing the contact angle of the material surface. The water absorption capacity of the material surface can be obtained by testing the contact angle of different films. First, the material is irradiated with visible light for at least 1 minute, so that the spiropyran molecules on the surface of the material are in a closed-loop state. At this time, the contact angle of the material surface is tested. Then the material is irradiated with a 365nm ultraviolet lamp for at least 30s, so that the spiropyran molecules on the surface of the material are all open-looped and transformed into hydrophilic partial indigo structures. At this time, the contact angle of the material surface is tested again, and it can be found that the contact angle becomes smaller, indicating that the hydrophilicity of the material surface is enhanced by ultraviolet light irradiation; at this time, the material is irradiated with visible light again to transform the partial indigo molecules on the surface into hydrophobic spiropyran molecules. At this time, the contact angle of the material surface is tested and it is found that the material restores the original contact angle value, indicating that ultraviolet-visible light has an important role in reversibly adjusting the water absorption-hydrophobicity of the material.

[0029] Step 5: Use a volume of 0.1m 3 The glass container simulates the microenvironment of humidity regulation. Before testing, the -2 m 2 (Film-area / container-volume ratio is 0.5m2 / m 3 ) film in a sealed glass container and left to stand until the temperature and humidity in the sealed container are constant. (It takes about 48 hours). Then place the UV lamp and visible light lamp outside the container, the purpose is to alternately provide light sources, especially to prevent the heating of the light source from affecting the test process. The entire test and humidity balance process is a light-proof environment to prevent any external light source from interfering with the test. Next, irradiate the film with UV light (wavelength 365nm), and the humidity in the sealed container will decrease until the humidity value remains unchanged. Similarly, continue to irradiate the film with visible light to increase the humidity value in the container.

[0030] In the embodiment, in order to adjust the maximum synergistic effect by changing the content of acrylic acid and methyl methacrylate, the humidity adjustment range of the material reaches the maximum value. Copolymers of acrylic acid and methyl methacrylate with different contents are prepared into films by electrospinning technology. The contact angle of the material and the humidity adjustment ability in a certain space are tested.

[0031] Example 1

[0032] Spiropyran copolymers were prepared by copolymerization of SPA, AA and MMA with AIBN as thermal initiator. In a 100 mL three-necked flask, 2.03 g (5.0 mmol) of SPA was dissolved in DMF (30 mL) under nitrogen atmosphere. The temperature was controlled at 65-70 ° C, and a mixed solution of 0 g AA and 5 g (50 mmol) of MMA was added. Under constant magnetic stirring, 0.50 g of AIBN was added and the solution was heated to 65-70 ° C. The polymerization was carried out under nitrogen atmosphere for 24 hours. After cooling to room temperature, the copolymer was precipitated in 100 mL of distilled water 3 times to remove unreacted monomers and residual initiator. The product was vacuum dried at 30 ° C for 12 hours to obtain a spiropyran copolymer.

[0033] The specific formula design of each component in this embodiment is shown in Table 1-1, and the test results of the contact angle and humidity adjustment range of the material are shown in Table 2. From the test data in Table 2, it can be seen that the material containing spiropyran on the surface does have the ability to adjust humidity.

[0034] Comparative Example 1

[0035] Acrylic acid was added during the copolymerization process, and the rest was the same as Example 1. By comparison, it can be seen that the contact angle of the material surface decreased after the addition of acrylic acid, indicating that the hydrophilicity of the material was enhanced, and when the material was alternately irradiated with ultraviolet-visible light, the contact angle variation range and humidity adjustment range of the material were also increased compared with Example 1, that is, the addition of acrylic acid did have a synergistic effect to enhance the adjustment ability.

[0036] Example 2

[0037] Spiropyran copolymers were prepared by copolymerization of SPA, AA and MMA with AIBN as thermal initiator. In a 100 mL three-necked flask, 2.03 g (5.0 mmol) of SPA was dissolved in DMF (30 mL) under nitrogen atmosphere. The temperature was controlled at 65-70 ° C, and a mixed solution of 0.36 g (5.0 mmol) of AA and 4.5 g (45 mmol) of MMA was added. Under constant magnetic stirring, 0.50 g of AIBN was added and the solution was heated to 65-70 ° C. The polymerization was carried out under nitrogen atmosphere for 24 hours. After cooling to room temperature, the copolymer was precipitated 3 times in 100 mL of distilled water to remove unreacted monomers and residual initiator. The product was vacuum dried at 30 ° C for 12 hours to obtain a spiropyran copolymer.

[0038] The specific formula design of each component in this embodiment is shown in Table 1-2, and the test results of the contact angle and humidity adjustment range of the material are shown in Table 2. It can be seen from the test data in Table 2 that the addition of acrylic acid significantly improves the water absorption capacity of the material surface and improves the humidity adjustment ability of the material.

[0039] Comparative Example 2

[0040] The content ratio of acrylic acid to methyl methacrylate was adjusted to seek the strongest synergistic effect and the largest humidity adjustment range. The other implementations were the same as Example 2. By comparison, it was found that changing the amount of acrylic acid added had a regular effect on the humidity adjustment range of the material.

[0041] Example 3

[0042] Spiropyran copolymers were prepared by copolymerization of SPA, AA and MMA with AIBN as thermal initiator. In a 100 mL three-necked flask, 2.03 g (5.0 mmol) of SPA was dissolved in DMF (30 mL) under nitrogen atmosphere. The temperature was controlled at 65-70 ° C, and a mixed solution of 0.72 g (10.0 mmol) of AA and 4 g (40 mmol) of MMA was added. Under constant magnetic stirring, 0.50 g of AIBN was added and the solution was heated to 65-70 ° C. The polymerization was carried out under nitrogen atmosphere for 24 hours. After cooling to room temperature, the copolymer was precipitated 3 times in 100 mL of distilled water to remove unreacted monomers and residual initiator. The product was vacuum dried at 30 ° C for 12 hours to obtain a spiropyran copolymer.

[0043] The specific formula design of each component in this embodiment is shown in Tables 1-3, and the test results of the contact angle and humidity adjustment range of the material are shown in Table 2. The test data in Table 2 show that changing the amount of acrylic acid added has a regular effect on the humidity adjustment range and contact angle.

[0044] Example 4

[0045] Spiropyran copolymers were prepared by copolymerization of SPA, AA and MMA with AIBN as thermal initiator. In a 100 mL three-necked flask, 2.03 g (5.0 mmol) of SPA was dissolved in DMF (30 mL) under a nitrogen atmosphere. The temperature was controlled at 65-70 ° C, and a mixed solution of 1.08 g (15.0 mmol) of AA and 3.5 g (35 mmol) of MMA was added. Under constant magnetic stirring, 0.50 g of AIBN was added and the solution was heated to 65-70 ° C. The polymerization was carried out under a nitrogen atmosphere for 24 hours. After cooling to room temperature, the copolymer was precipitated 3 times in 100 mL of distilled water to remove unreacted monomers and residual initiator. The product was vacuum dried at 30 ° C for 12 hours to obtain a spiropyran copolymer.

[0046] The specific formula design of each component in this embodiment is shown in Tables 1-4, and the test results of the contact angle and humidity adjustment range of the material are shown in Table 2. The test data in Table 2 show that changing the amount of acrylic acid added has a regular effect on the humidity adjustment range and contact angle.

[0047] Example 5

[0048] Spiropyran copolymers were prepared by copolymerization of SPA, AA and MMA with AIBN as thermal initiator. In a 100 mL three-necked flask, 2.03 g (5.0 mmol) of SPA was dissolved in DMF (30 mL) under nitrogen atmosphere. The temperature was controlled at 65-70 ° C, and a mixed solution of 1.44 g (20.0 mmol) of AA and 3.0 g (30 mmol) of MMA was added. Under constant magnetic stirring, 0.50 g of AIBN was added and the solution was heated to 65-70 ° C. The polymerization was carried out under nitrogen atmosphere for 24 hours. After cooling to room temperature, the copolymer was precipitated 3 times in 100 mL of distilled water to remove unreacted monomers and residual initiator. The product was vacuum dried at 30 ° C for 12 hours to obtain a spiropyran copolymer.

[0049] The specific formula design of each component in this embodiment is shown in Tables 1-5, and the test results of the contact angle and humidity adjustment range of the material are shown in Table 2. The test data in Table 2 show that changing the amount of acrylic acid added has a regular effect on the humidity adjustment range and contact angle.

[0050] Table 2 Contact angle variation range and humidity regulation ability of each group of materials in the embodiment

[0051] example Initial contact angle (°) Contact angle change (°) Humidity adjustment range (%) 1 146.3 8.4 5.2 2 140.1 13.5 9.0 3 136.8 18.6 12.5 4 128.5 14.6 10.1 5 119.8 10.2 6.9

Claims

1. A method for preparing a synergistically enhanced light-controlled humidity-regulating fiber membrane, Features: The preparation method comprises: the first step of synthesizing spiropyran monomer molecules, dissolving 2,3,3-trimethyl-3H-indole and 2-bromoethanol in anhydrous CH 3 CN, 2,3,3-trimethyl-3H-indole:2-bromoethanol = 1:1-1:1.5, n:n, to form a red solution; the red solution was refluxed and stirred under a nitrogen atmosphere until it cooled to room temperature; the solvent was evaporated in vacuum to anhydrous CH 3 CN, obtain a crude product; the crude product is recrystallized with acetone and washed with acetone to obtain compound 1, which is a light pink solid compound 1; compound 1 and 5-nitrosalicylicylaldehyde are dissolved in anhydrous ethanol, compound 1:5-nitrosalicylicylaldehyde=1:1-1:1.2, n:n, heated to reflux, diethylamine is added and the mixture is refluxed under nitrogen, cooled to room temperature, and anhydrous ethanol is removed in vacuo to obtain a solid; the obtained solid is washed with distilled water, and then chromatographed on a silica gel column using an ethyl acetate / petroleum ether mixture with a volume ratio of 1 / 5 v / v as an eluent to produce compound 2. Compound SP-OH, SP-OH is a purple needle-shaped product; SP-OH and anhydrous dichloromethane are added to a round-bottom flask, the solution is stirred at 0-5°C to completely dissolve SP-OH, and then acryloyl chloride is added dropwise to the mixed solution of SP-OH and anhydrous dichloromethane under a nitrogen atmosphere, and triethylamine is added dropwise while stirring continuously to form a mixture, SPOH: acryloyl chloride: triethylamine = 1:1:1-1:1.5:1.5, n:n:n, the mixture is refluxed at low heat and the solvent is removed using a rotary evaporator, and the obtained solid is washed with dichloromethane and extracted multiple times; the solid is chromatographed on a silica column using an ethyl acetate / petroleum ether mixture with a volume ratio of 1 / 5 v / v as an eluent to obtain a light yellow solid spiropyran monomer molecule SPA; Step 2: The spiropyran monomer SPA obtained in the first step is copolymerized with acrylic acid AA and methyl methacrylate MMA using AIBN as a thermal initiator to prepare a spiropyran copolymer; SPA is dissolved in DMF in a three-necked flask under a nitrogen atmosphere; the temperature is controlled at 65-70°C, and a mixed solution of AA and MMA in a certain proportion is added, SPA:AA:MMA=1:1:9-1:4:6, n:n:n; AIBN is added under constant magnetic stirring and the solution is heated to 65-70°C; polymerization is carried out under a nitrogen atmosphere; after cooling to room temperature, the copolymer is precipitated in distilled water to remove unreacted monomers and residual initiator, and the product is obtained; the product is vacuum dried to obtain the spiropyran copolymer; Step 3: Prepare spiropyran copolymers with different ratios of AA and MMA into a DMF solution with a concentration of 45 wt%; the ambient temperature and relative humidity of the electrospinning process are maintained at 24±1℃ and 20±2%, respectively; connect the electrospinning needle to a high-voltage power supply and apply a stable voltage; finally, dry the electrospun film under vacuum to prepare a membrane material with adjustable humidity.