Amorphous silicon / hard carbon composite materials and their preparation and application in lithium-ion batteries

By filling the pore structure of hard carbon particles with amorphous silicon and using negative pressure-positive pressure control and microwave-assisted reaction processes, the problems of low specific capacity and low first efficiency of hard carbon anode materials are solved, and high capacity and high first efficiency are achieved. The efficient amorphous silicon/hard carbon composite material significantly improves the rapid charge and discharge capability and electrochemical performance of lithium-ion batteries.

CN115832267BActive Publication Date: 2024-10-11NANNING CHENYU NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111089364.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-16
Publication Date
2024-10-11
Estimated Expiration
2041-09-16

AI Technical Summary

Technical Problem

The problems of hard carbon anode materials in lithium-ion batteries include low specific capacity, low first efficiency, and the inability to achieve rapid lithium ion deintercalation, which limits its fast charge and discharge performance and wide application.

Method used

Using amorphous silicon/hard carbon composite materials, by filling the pore structure and defects of hard carbon particles with amorphous silicon, combined with negative pressure-positive pressure control and microwave-assisted reaction processes, a high-capacity and high-efficiency composite materials.

Benefits of technology

It significantly improves the rapid deintercalation ability of lithium ions and the electrochemical performance of the battery, increases the material's capacity and first Coulomb efficiency, and achieves excellent fast charging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115832267B_ABST
    Figure CN115832267B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of negative electrode materials for lithium secondary batteries, and specifically discloses an amorphous silicon / hard carbon composite material, including hard carbon particles and amorphous silicon filled in the pore structure and / or defects of the hard carbon particles. The present invention also discloses a variable voltage microwave assisted reaction preparation process of the material and its application in lithium secondary batteries. The present invention has found that innovatively filling amorphous silicon in the pores and defects of hard carbon can reduce the impedance of the material, improve the transfer rate of active ions, significantly enhance the ability to quickly deintercalate lithium, improve the capacity and initial efficiency of the material, and assemble the material into a battery to improve the performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of negative electrode materials, and in particular relates to a new lithium ion amorphous silicon / hard carbon composite negative electrode active material. Background Art

[0002] Now is an era of the rise of new energy. As a high-energy-density secondary battery, lithium-ion batteries play an important role in the application of more and more new energy sources such as electrification and cordless. Lithium-ion batteries realize the function of charge transfer and charging and discharging by the continuous shuttling of lithium ions between the positive and negative electrodes. They are mainly assembled through a series of component components such as positive and negative electrode materials, diaphragms, and electrolytes. Kinetic performance is a very important performance of positive and negative electrodes. It mainly refers to the ability of lithium ions to quickly embed and detach, thereby realizing the ability of batteries to charge and discharge quickly. There are two main aspects that affect kinetic performance: one is the entire electrode level. The thickness of the electrode coating means the distance of the lithium ion transmission path. The shorter the path, the easier it is to transmit quickly; the other is the material level. The ability of the electrode material itself to quickly intersperse lithium ions also contributes greatly to the kinetic performance. At present, the negative electrode material of commercial lithium-ion batteries is mainly graphite, including natural graphite and artificial graphite. Graphite is a highly ordered layered structure. Lithium ions are mainly stored in the gaps between graphite layers. Lithium ions are directional when embedded and released. When the battery is rapidly charged and discharged, lithium ions cannot penetrate from a certain direction in time, which can easily cause lithium precipitation, thus causing the battery to short-circuit or even explode. Therefore, the dynamic performance of graphite still needs to be improved. Due to technical problems, the lack of rapid charge and discharge capability is still one of the major bottlenecks restricting the development of lithium-ion batteries.

[0003] Among carbon materials, hard carbon has better kinetic properties. According to literature reports (Research Progress of Hard Carbon Anode Materials for Lithium-ion Batteries [J]. Materials Guide, 2017, 031(001): P.236-241.), hard carbon is a kind of carbon that is difficult to graphitize. Due to its amorphous microstructure, it is Li + The diffusion transport inside the material provides a wide channel, which is beneficial to improve the charge and discharge performance of the material under high current. However, hard carbon is generally made by carbonizing materials such as resins or biomass. Its microstructural characteristics will increase impedance, restrain or hinder the transmission of lithium ions, and affect the ability of hard carbon itself to charge and discharge quickly. In addition, it will also generate a large amount of solid electrolyte interface layer (SEI film) in the battery electrolyte, resulting in an increase in the first irreversible capacity and a decrease in the first coulomb efficiency, which also reduces the actual energy density of the battery and is not conducive to fast charging performance at the electrode level. The first efficiency of commercial hard carbon is generally lower than <82%, which is one of the main reasons why hard carbon cannot be widely used directly in lithium-ion batteries.

[0004] The patent (CN108963253) proposes a method for preparing porous hard carbon negative electrode materials, and obtains a hard carbon negative electrode with an initial coulombic efficiency of 84%. The patent does not report its kinetic data, and the initial efficiency of 84% is still far from the initial efficiency requirement of more than 90% for general negative electrodes.

[0005] In summary, although hard carbon has the potential for fast charging and discharging, it is difficult to realize its fast charging potential due to its microstructural characteristics. It still has problems such as low specific capacity, low initial efficiency, and inability to achieve rapid lithium ion deintercalation. Summary of the invention

[0006] In order to solve the problems of low specific capacity, low initial efficiency, and inability to realize rapid lithium ion deintercalation of hard carbon, the first purpose of the present invention is to provide an amorphous silicon / hard carbon composite material, aiming to provide a composite negative electrode active material with both high capacity and high initial efficiency.

[0007] The second object of the present invention is to provide a method for preparing the amorphous silicon / hard carbon composite material.

[0008] The third object of the present invention is to provide the use of the amorphous silicon / hard carbon composite material as a negative electrode active material.

[0009] The fourth object of the present invention is to provide a lithium ion battery containing the amorphous silicon / hard carbon composite material.

[0010] An amorphous silicon / hard carbon composite material comprises hard carbon particles and amorphous silicon filled in the pore structure and / or defects of the hard carbon particles.

[0011] The present invention has found that innovatively filling the pores and defects of hard carbon with amorphous silicon can reduce the impedance of the material, improve the transfer rate of active ions, significantly enhance the ability to quickly deintercalate and deintercalate lithium, improve the capacity and initial efficiency of the material, and assemble the material into a battery to improve the performance of the battery.

[0012] In the present invention, the hard carbon and amorphous silicon phases and the structural characteristics of amorphous silicon filling hard carbon pores and defects are the key to synergistically improving the capacity and first efficiency of the composite material and improving battery performance. The study also found that further control of the hard carbon structure and the content of amorphous silicon can help further improve the electrochemical properties of the composite material, such as capacity and first efficiency.

[0013] In the present invention, the hard carbon is a carbon material that is difficult to graphitize at a high temperature of 2000° C. or above.

[0014] Preferably, the hard carbon particles have a microporous and / or mesoporous pore structure. That is, the pore size of the pore structure in the hard carbon particles is ≤50nm. Studies have found that the control of the pore structure is conducive to the electrochemical performance of the composite material.

[0015] Preferably, the specific surface area of ​​the hard carbon particles is 100-300m 2 / g, preferably 190 to 260 m 2 / g;

[0016] Preferably, the D50 of the hard carbon particles is 1-20 microns, preferably 3-10 microns;

[0017] Preferably, the pore volume of the hard carbon particles is 20-30%, more preferably 22-29%, and even more preferably 26-29%.

[0018] In the present invention, the filling rate of the amorphous silicon on the pore structure and / or defects of the hard carbon particles is greater than or equal to 90%;

[0019] Preferably, the amorphous silicon is also allowed to be compounded on the particle surface of the hard carbon particles;

[0020] Preferably, the amorphous silicon / hard carbon composite material is composed of hard carbon particles and amorphous silicon filled in the pore structure and / or defects of the hard carbon particles;

[0021] Preferably, in the amorphous silicon / hard carbon composite material, the content of amorphous silicon is less than or equal to 10 wt.%, preferably 4 to 8 wt.%, and more preferably 6 to 7.5%.

[0022] Preferably, the amorphous silicon / hard carbon composite material has a specific surface area less than or equal to 10 m 2 / g, for example, can be 3.5 to 5.5 m 2 The pore volume is less than or equal to 3%, for example, it may be 1 to 2%.

[0023] The mass specific capacity of the amorphous silicon / hard carbon composite material of the present invention is 450-650 mAh / g, and the first coulombic efficiency is ≥90%.

[0024] The present invention also provides a method for preparing the amorphous silicon / hard carbon composite material, wherein hard carbon particles are placed in a reaction device (reaction chamber), the pressure of the reaction device is controlled to be negative pressure, silicon source gas is then introduced into the reaction device to make the pressure in the reaction device positive pressure, and then microwave heating is performed to react at 450-550°C to obtain the amorphous silicon / hard carbon composite material.

[0025] The present invention has found that in order to successfully prepare the material, it is necessary to solve the problems of amorphous silicon phase purity and heterogeneous nucleation outside the amorphous silicon pores. In response to this preparation problem, the present invention has found through research that the formation of crystalline silicon can be unexpectedly avoided and the phase purity of amorphous silicon can be improved by innovatively using the negative pressure-positive pressure combined pressure control-microwave assisted reaction process, and further coordinating the microwave assisted reaction temperature. Not only that, it can also solve the heterogeneous nucleation of amorphous silicon and achieve effective filling of the pores and defects of amorphous silicon, thereby reducing the impedance of the prepared material, improving the transfer rate of active ions, improving the capacity and first efficiency of the material, and improving the electrochemical properties of the material.

[0026] In the present invention, the combined synergy of the negative pressure-positive pressure control means and the microwave-assisted reaction means is the key to improving the amorphous silicon phase and the amorphous silicon pore filling rate, and improving the performance of the obtained material.

[0027] Preferably, the negative pressure is ≤1pa.

[0028] The silicon source gas is a silicon-containing gas, preferably at least one of silane (SiH4), trichlorosilane (SiHCl3), and dichlorosilane (SiH2Cl2).

[0029] The positive pressure is 1-10MPa.

[0030] Preferably, the frequency of the microwaves is 1500-2500 MHz.

[0031] Preferably, the reaction temperature is 500-550°C.

[0032] In the present invention, the reaction time is 5-20 min, preferably 10-15 min.

[0033] In the present invention, after the reaction is completed and the temperature is lowered to room temperature, the residual silicon source gas is completely removed with nitrogen and the silicon source gas is burned by a tail gas treatment device, and then the reaction equipment is opened to obtain the desired composite material.

[0034] The present invention also provides the application of the amorphous silicon / hard carbon composite material, which is used as a negative electrode active material;

[0035] Preferably, it is used as a negative electrode active material for lithium ion batteries.

[0036] The application described in the present invention can be based on existing means, using the amorphous silicon / hard carbon composite material as a negative electrode active material to prepare a negative electrode material, a negative electrode sheet, and a lithium-ion battery.

[0037] For example, the amorphous silicon / hard carbon composite material is used as a negative electrode active material, slurried with a known conductive agent, a binder and a solvent to form a negative electrode slurry, and then coated and dried on the surface of the current collector to obtain a negative electrode sheet, which is then assembled into a lithium-ion battery with a conventional positive electrode sheet, a separator and an electrolyte.

[0038] The present invention also provides a lithium ion battery, the negative electrode of which comprises the amorphous silicon / hard carbon composite material.

[0039] The lithium-ion battery of the present invention, except that the negative electrode active material is the amorphous silicon / hard carbon composite material of the present invention, the other materials and structures thereof may be known.

[0040] Beneficial effects:

[0041] 1. The present invention provides a new amorphous silicon / hard carbon composite material, and it is found that through the joint control of the amorphous phase and structure of the material, the impedance of the material can be synergistically reduced, providing a large number of channels for the transmission of active ions such as (Li+); improving the rapid migration ability of active ions, improving the capacity and initial efficiency of the material; assembling it into a battery is helpful to obtain a battery with excellent electrochemical properties, especially excellent fast charging performance.

[0042] The material of the present invention exhibits higher specific capacity and first coulombic efficiency, so that under the same capacity design, the negative electrode coating is thinner, which is further beneficial to improving the rapid charge and discharge capability of the battery.

[0043] 2. Through the control of the negative-positive pressure transformation means and microwave-assisted reaction means and conditions, the amorphous phase of silicon can be controlled, and the heterogeneous nucleation of amorphous silicon can be avoided, the formation of free silicon can be avoided, and the filling of hard carbon pores and defect structures by amorphous silicon can be improved, thereby helping to reduce the impedance of the prepared material, improve the capacity and first efficiency, and improve the performance of the assembled battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is the XRD spectrum of the material prepared in Example 1. It can be seen that XRD shows a hard carbon package, and since silicon is amorphous silicon, XRD does not show a silicon peak. DETAILED DESCRIPTION

[0045] The present invention will be described in detail below with reference to the embodiments, but the present invention is not limited thereto.

[0046] Example 1

[0047] First, 100 g of hard carbon with a particle size D50 of 20 microns and a specific surface area of ​​120 m2 / g was taken, and the interior was mainly micropores and mesopores. The volume ratio of the test pores (pore volume) was 22%.

[0048] Then, the hard carbon material was placed in a rotary furnace with microwave heating function, and the furnace was evacuated to 0.5Pa at room temperature, and then silane (SiH4) gas was introduced to reach 2MPa. Then microwave heating (microwave frequency was 1500MHz) was started to 475℃ and kept warm for 10 minutes, and then the temperature was lowered. After cooling to room temperature, the residual silane was completely removed with nitrogen and the silane was burned by the tail gas treatment device, and then the furnace was opened to obtain the desired composite material (XRD see Figure 1 ). According to the test, the composite material has a specific surface area of ​​3.5 m2 / g, a pore volume of 1.3%, and an amorphous silicon content of 4.5 wt.%.

[0049] Example 2

[0050] First, 100 g of hard carbon with a particle size D50 of 10 microns and a specific surface area of ​​190 m2 / g was taken, and the interior was mainly micropores and mesopores. The tested pore volume was 26%.

[0051] Then, the hard carbon material is placed in a rotary furnace with microwave heating function, the furnace is evacuated to 0.1Pa at room temperature, and then silane (SiH4) gas is introduced to reach 5MPa. Then microwave heating (microwave frequency is 2000MHz) is started to 500℃ and kept warm for 10 minutes, and then the temperature is lowered. After cooling to room temperature, the residual silane is completely removed with nitrogen and the silane is burned out using an exhaust gas treatment device, and then the furnace is opened to obtain the required composite material (having a physical phase similar to that in Example 1). After testing, the composite material has a specific surface of 4.8m2 / g, a pore volume of 1.6%, and an amorphous silicon content of 6.3%.

[0052] Example 3

[0053] Take 100g of hard carbon with a particle size of 3 microns and a specific surface area of ​​260m2 / g, the interior of which is mainly micropores and mesopores. The tested pore volume is 29%.

[0054] Then, the hard carbon material is placed in a rotary furnace with microwave heating function, the furnace is evacuated to 0.05Pa at room temperature, and then silane (SiH4) gas is introduced to reach 10MPa. Then microwave heating (microwave frequency is 2500MHz) is started to 550℃ and kept warm for 10 minutes, and then the temperature is lowered. After cooling to room temperature, the residual silane is completely removed with nitrogen and the silane is burned out using an exhaust gas treatment device, and then the furnace is opened to obtain the required composite material (having a physical phase similar to that in Example 1). After testing, the composite material has a specific surface of 5.2m2 / g, a pore volume of 1.8%, and an amorphous silicon content of 7.2%.

[0055] Comparative Example 1

[0056] Compared with Example 2, the only difference is that no amorphous silicon filling is performed.

[0057] Take 100g of the same hard carbon as in Example 2 and place it in a rotary furnace with microwave heating function. Pump the furnace to 0.1Pa at room temperature. Then start microwave heating with a microwave frequency of 2000MHz, raise the temperature to 500℃, keep the temperature for 10 minutes and then cool it down. After cooling to room temperature, open the furnace to obtain the desired composite material.

[0058] Comparative Example 2

[0059] Compared with Example 2, the only difference is that the filled amorphous silicon is converted into crystalline silicon, for example:

[0060] The composite material obtained in Example 2 was heated to 800° C. under vacuum conditions and kept at this temperature for 2 hours to transform the amorphous silicon into crystalline silicon.

[0061] Comparative Example 3

[0062] Compared with Example 2, the only difference is that hard carbon with a macroporous structure is used, specifically:

[0063] First, 100 g of hard carbon material with a particle size D50 of 10 micrometers and mainly macropores larger than 50 nm was taken, and the test pore volume was 30%.

[0064] Then, the hard carbon material is placed in a rotary furnace with microwave heating function, the furnace is evacuated to 0.1Pa at room temperature, and then silane (SiH4) gas is introduced to reach 5MPa. Then microwave heating is started, the microwave frequency is 2000MHz, the temperature rises to 500℃, and then it is kept warm for 10 minutes and then cooled. After cooling to room temperature, the residual silane is completely removed with nitrogen and the silane is burned by the tail gas treatment device, and then the furnace is opened to obtain the desired composite material.

[0065] Comparative Example 4

[0066] Compared with Example 2, the only difference is that no negative pressure treatment is performed in advance, specifically:

[0067] Take 100g of the same hard carbon material as in Example 2 and place it in a rotary furnace with microwave heating function, replace the gas in the furnace with argon, keep the argon at normal pressure, and then introduce silane (SiH4) gas to reach 5MPa. Then start microwave heating, the microwave frequency is 2000MHz, the temperature rises to 500℃, keeps warm for 10 minutes and then cools down. After cooling to room temperature, the residual silane is completely removed with nitrogen and the silane is burned by the tail gas treatment device, and then the furnace is opened to obtain the desired composite material.

[0068] Comparative Example 5

[0069] Compared with Example 2, the only difference is that the microwave-assisted reaction is not performed, specifically:

[0070] 100 g of the same hard carbon material as in Example 2 was placed in a rotary furnace heated by a resistance wire, and the pressure in the furnace was set to 0.1 Pa, and then silane (SiH4) gas was introduced to reach 5 MPa. Then the heating was started and raised to 500°C, and then the temperature was kept for 10 minutes, and then the temperature was lowered. After the temperature dropped to room temperature, the residual silane was completely removed with nitrogen and the silane was burned by an exhaust gas treatment device, and then the furnace was opened to obtain the desired composite material.

[0071] Comparative Example 6

[0072] Compared with Example 2, the only difference is that the temperature of the microwave reaction is 400° C., specifically:

[0073] Take 100g of the same hard carbon material as in Example 2 and place it in a rotary furnace with microwave heating function. Pump the furnace to 0.1Pa, and then introduce silane (SiH4) gas to reach 5MPa. Then start microwave heating with a microwave frequency of 2000MHz. After the temperature rises to 400℃, keep it warm for 10 minutes and then cool it down. After cooling to room temperature, the remaining silane is completely removed with nitrogen and the silane is burned out using an exhaust gas treatment device, and then the furnace is opened to obtain the required material. After testing, due to the low heating temperature, the decomposition rate of silane is extremely low, and there is basically no silicon element in the resulting material.

[0074] Comparative Example 7

[0075] Compared with Example 2, the only difference is that the temperature of the microwave reaction is 600° C., specifically:

[0076] Take 100g of the same hard carbon material as in Example 2 and place it in a rotary furnace with microwave heating function. Pump the furnace to 0.1Pa, then introduce silane (SiH4) gas to 5MPa. Then start microwave heating, the microwave frequency is 2000MHz, the temperature rises to 600℃, keeps warm for 10 minutes and then cools down. After cooling to room temperature, the residual silane is completely removed with nitrogen and the silane is burned by the tail gas treatment device, and then the furnace is opened to obtain the desired material.

[0077] Performance Testing

[0078] The electrode materials prepared in the above-mentioned embodiments 1 to 3 and the comparative examples 1 to 7 are made into electrode slurry. The slurry ratio is electrode material: binder (PAA): conductive agent (SP) = 75:15:10. After the slurry is stirred evenly, it is coated on the copper foil and then dried under vacuum. The dried electrode sheet is used as the working electrode of the button battery, the lithium sheet is used as the counter electrode, and the electrolyte is 1 mol / L lithium hexafluorophosphate (LiPF6) electrolyte dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) electrolyte with a volume ratio of 1:1. The first lithium delithiation specific capacity and the first coulomb efficiency of the above-mentioned material are tested at a current density of 0.2C, and the current of 0.5C and 10C is continued to be used to test its capacity, and the ratio of the capacity at 10C and 0.5C is used as an indicator of its rapid charge and discharge performance. The larger the value, the stronger the rapid charge and discharge ability of the material. The constant current charge and discharge voltage range is 0.01-1.5V.

[0079] As can be seen from Table 1, Examples 1-3 all show higher first lithium removal specific capacity, higher first coulombic efficiency, and 10C / 0.5C capacity than Comparative Example 1. Example 2 and Comparative Example 2 are comparisons between amorphous silicon and crystalline silicon, and amorphous silicon shows a higher 10C / 0.5C capacity ratio than crystalline silicon. It can be seen that the negative electrode material of this patent invention does show high kinetic performance.

[0080] Table 1: Test results of examples and comparative examples

[0081]

[0082] In summary, through the negative-positive pressure transformation means and the control of microwave-assisted reaction means and conditions, the amorphous phase of silicon can be controlled, and the heterogeneous nucleation of amorphous silicon can be avoided, the formation of free silicon can be avoided, and the filling of hard carbon pores and defect structures by amorphous silicon can be improved, which helps to reduce the impedance of the prepared material, improve the capacity and first effect, and improve the performance of the assembled battery.

Claims

1. A method for preparing an amorphous silicon / hard carbon composite material, It is characterized in that The preparation method is as follows: placing hard carbon particles in a reaction device, controlling the pressure of the reaction device to be negative pressure, then introducing silicon source gas into the reaction device to make the pressure in the reaction device positive pressure, then microwave heating to 450-550°C for reaction to obtain the amorphous silicon / hard carbon composite material; the hard carbon particles have a microporous and / or mesoporous pore structure; the negative pressure is ≤1Pa; and the positive pressure is 1-10MPa.

2. The method according to claim 1, It is characterized in that The specific surface area of ​​the hard carbon particles is 100-300m 2 / g; the D50 of the hard carbon particles is 1-20 microns; the pore capacity of the hard carbon particles is 20-30%.

3. The method according to claim 1, It is characterized in that The filling rate of the amorphous silicon on the pore structure and / or defects of the hard carbon particles is greater than or equal to 90%; the amorphous silicon is also allowed to be compounded on the surface of the hard carbon particles; the specific surface area of ​​the amorphous silicon / hard carbon composite material is ≤10m 2 / g; the pore volume of the amorphous silicon / hard carbon composite material is ≤3%; the amorphous silicon / hard carbon composite material is composed of hard carbon particles and amorphous silicon filled in the pore structure and / or defects of the hard carbon particles; in the amorphous silicon / hard carbon composite material, the content of amorphous silicon is less than or equal to 10wt.%.

4. The method according to claim 3, It is characterized in that The content of amorphous silicon is 4-8 wt.%.

5. The method according to claim 1, It is characterized in that The silicon source gas is a gas containing silicon.

6. The method according to claim 1, It is characterized in that The silicon source gas is at least one of silane, trichlorosilane and dichlorosilane.

7. The method according to claim 1, It is characterized in that The reaction time is 5-20 min; the microwave frequency is 1500-2500 MHz.

8. Use of an amorphous silicon / hard carbon composite material prepared by the preparation method according to any one of claims 1 to 7, It is characterized in that It is used for negative electrode active material.

9. The use according to claim 8, It is characterized in that Specifically, it is used as negative electrode active material for lithium-ion batteries.

10. A lithium ion battery, It is characterized in that The negative electrode comprises an amorphous silicon / hard carbon composite material prepared by the preparation method according to any one of claims 1 to 7.