Annealing method for glass aspherical lens

By loading materials on the hollow bracket and passing inert gas to control multiple temperature changes, the problem of improper annealing temperature of the glass aspherical lens is solved, uniform heating of the lens and elimination of thermal stress are achieved, and the optical performance and annealing quality of the lens are improved. .

CN115849689BActive Publication Date: 2024-10-25XIAMEN FULI OR MU PHOTOELECTRIC TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211378500.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-10-25
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

In the existing annealing process of glass aspherical lenses, the annealing temperature is often too low or too high, leading to problems such as insufficient annealing, lens deformation, surface fogging or explosion.

Method used

An annealing method for glass aspherical lenses is adopted, which includes loading materials on a hollow support, passing in inert gas, controlling the temperature through heating, insulation, and multiple cooling processes in sequence, and using circulating hot air during the annealing process to ensure that the lens is heated evenly , the cooling rate gradually increases, and finally cools naturally.

Benefits of technology

Effectively eliminate the thermal stress of the lens, restore optical constants, improve surface shape errors, improve the overall annealing effect and efficiency of the lens, prevent surface fogging, and ensure product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115849689B_ABST
    Figure CN115849689B_ABST
Patent Text Reader

Abstract

This patent relates to the field of lens annealing, specifically, to an annealing method for a glass aspheric lens, comprising the following steps: S1 placing the lens in an annealing furnace; S2 introducing an inert gas into the furnace; S3 annealing: controlling the temperature to sequentially undergo a heating process, a heat preservation process, a primary cooling process, a secondary cooling process, and a tertiary cooling process; S31 setting the initial temperature to T0, heating to a heat preservation temperature T1 at a rate of 2.5-4°C / min; S32 heat-insulating the glass aspheric lens at T1; S33 cooling the temperature T1 to T2 at a rate of 0.3-0.7°C / min; S34 cooling the temperature T2 to T3 at a rate of 0.8-1.2°C / min; S35 cooling the temperature T3 to T4 at a rate of 1.3-2°C / min; S4 taking the material for inspection, introducing an inert gas during the annealing process to prevent the lens from fogging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This patent relates to the field of lens annealing, and specifically, to a method for annealing a glass aspherical lens. Background Art

[0002] Aspheric lenses have high requirements for aspheric shape error, geometric dimensions, refractive index, dispersion coefficient, and stress. Since optical glass materials undergo drastic temperature changes and shape changes during the molding process, their refractive index and dispersion coefficient have changed, leaving thermal stress. Annealing is an important process to restore the refractive index value of the lens after molding, eliminate residual thermal stress, stabilize aspheric shape error, improve lens strength, etc., and meet the technical requirements of the drawings.

[0003] The current annealing process mainly includes the annealing process directly in the furnace after the forming process of the multi-axis forming equipment, which is called the primary annealing; and after the forming is cooled, it is heated and annealed in a special annealing furnace, which is called the secondary annealing. The time of the primary annealing is relatively short, which can easily cause insufficient annealing of the lens, so that the thermal internal stress cannot be effectively released, and the optical constants deviate from the design value, and then a secondary annealing is required. The existing annealing process often has the problem of the annealing temperature being too low or too high or the temperature rising and falling being too fast. The annealing temperature is too low, resulting in insufficient annealing, and the annealing temperature is too high, resulting in the free position of the lens particles at high temperature, causing product deformation, surface fogging, or the lens bursting due to too fast temperature rising and falling. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention provides an annealing method for a glass aspherical lens, which can solve the problems of the existing annealing process such as the annealing temperature being too low or too high. The annealing temperature is too low, resulting in insufficient annealing; the annealing temperature is too high, resulting in the free position of the lens particles at high temperature, causing product deformation, surface fogging, or the lens bursting due to too fast heating and cooling.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for annealing a glass aspherical lens, characterized in that it comprises the following steps:

[0007] S1 Loading: Arrange the molded lenses on the hollow bracket, place the hollow bracket in the annealing furnace, and close the furnace door;

[0008] S2 ventilation: Inert gas is introduced into the annealing furnace so that the volume proportion of oxygen in the annealing furnace is less than 0.8%;

[0009] S3 annealing: the temperature is controlled to go through a heating process, a heat preservation process, a first cooling process, a second cooling process and a third cooling process in sequence;

[0010] S31: the heating process: assuming the initial temperature to be T0, heating to the insulation temperature T1 at a rate of 2.5-4°C / min;

[0011] S32: the heat preservation process: heat the glass aspherical lens at a temperature of T1 for a heat preservation time of t;

[0012] S33: the first cooling process: cooling the temperature from T1 to T2 at a rate of 0.3-0.7°C / min;

[0013] S34: the second cooling process: cooling the temperature from T2 to T3 at a rate of 0.8-1.2°C / min;

[0014] S35: the third cooling process: cooling the temperature T3 to the temperature T4 at a rate of 1.3-2°C / min;

[0015] S4 Material inspection: Open the furnace door, take out the glass aspheric lens, and inspect the residual thermal stress, aspheric surface error, refractive index, dispersion coefficient, center thickness, outer diameter and surface appearance of the glass aspheric lens.

[0016] Furthermore, in step S2, the inert gas is nitrogen or argon.

[0017] Furthermore, in step S2, the ventilation flow rate of the inert gas is greater than 200 mL / min.

[0018] Furthermore, in step S31, T1=(Ta+Tstp) / 2, Ta is the annealing point temperature of the glass aspherical lens material, and Tstp is the strain point temperature of the glass aspherical lens material.

[0019] Furthermore, in step S33, T2=Tstp-100°C.

[0020] Furthermore, in step S34, T3=Tstp-200°C.

[0021] Furthermore, in step S35, the temperature of T4 is 50-100°C.

[0022] Furthermore, in step S3, the annealing process uses circulating hot air to heat the annealing furnace.

[0023] Furthermore, the method further includes step S36, in which when the temperature reaches T4, the addition of the inert gas is turned off, the heating of the annealing furnace is stopped, the furnace door is opened to a 1 / 3 position, and the annealing furnace is allowed to cool naturally to room temperature.

[0024] Further, in step S32, the holding time t=α·η·D+60, wherein α is the heating coefficient (min / mm), η is the correction coefficient of the furnace loading condition; and D is the maximum thickness of the aspherical lens (mm).

[0025] The beneficial effects of the present invention are:

[0026] 1. In this solution, the lens is placed on the annealing plate, and the annealing plate is fixed on a matching annealing rack, which improves the utilization rate of the space in the annealing furnace, makes the upper and lower surfaces of the lens on the annealing plate heated evenly, and thus improves the overall annealing effect of the lens.

[0027] 2. In this scheme, the cooling process in annealing is segmented, and the cooling rates of the first cooling process, the second cooling process and the third cooling process are increased successively. This can effectively eliminate the thermal stress of the lens during the molding process, restore the designed optical constants, and improve the surface error. While ensuring the quality of lens annealing, efficiency is taken into account.

[0028] 3. In this solution, an oxygen-free environment is created by introducing inert gas during the annealing process, which prevents the residual oxygen in the annealing furnace from reacting with the lens and can effectively control the fogging of the lens surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 A schematic flow chart of the aspheric lens annealing method of the present invention;

[0031] Figure 2 Annealing curve diagram of the aspheric lens annealing method of the present invention;

[0032] Figure 3 A schematic diagram of the structure of the lens according to Embodiment 1 of the present invention;

[0033] Figure 4 The time-temperature curve diagram of Example 1 of the present invention;

[0034] Figure 5 A schematic diagram of the hollow material frame structure of the present invention;

[0035] Figure 6 Schematic diagram of the structure of the annealing plate and annealing tray according to the present invention.

[0036] Main component symbols

[0037] 1. Hollow bracket; 101. Side plate; 102. Top plate; 103. Bottom plate; 104. Ventilation hole; 105. Guide groove;

[0038] 2. Annealing plate; 201. Installation channel;

[0039] 3. Lenses;

[0040] 4. Annealing tray. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the invention claimed for protection, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0042] Please refer to Figure 1-6 The present invention provides a method for annealing a glass aspherical lens, comprising the following steps:

[0043] S1 Loading: Arrange the molded lenses 3 on the hollow bracket 1, place the hollow bracket 1 in the annealing furnace, and close the furnace door; please refer to Figure 5 and 6 , wherein the hollow bracket 1 includes two opposite side panels 101 and a top panel 102 and a bottom panel 103 fixed to the top and bottom of the side panels 101, and a plurality of vent holes 104 arranged in an array are provided on the side panels 101, the top panel 102 and the bottom panel 103. A corresponding guide groove 105 is provided on the opposite sides of the two side panels 101, and the guide groove 105 is used to install the annealing plate 2, and a plurality of installation channels arranged in an array are provided on the annealing plate 2, and the glass aspherical lens 3 is placed in the installation channel.

[0044] S2 ventilation: Introduce inert gas into the annealing furnace so that the volume proportion of oxygen in the annealing furnace is less than 0.8%, so that the lens 3 is in an inert gas atmosphere during the annealing process, avoiding the reaction between the lens 3 and oxygen and other gases in the air, and effectively controlling the fogging of the surface of the lens 3; wherein the inert gas is nitrogen or argon, and the ventilation flow rate of the inert gas is 200-500mL / min, and the ventilation flow rate of the inert gas is preferably controlled at 300-350mL / min;

[0045] S3 annealing: the temperature is controlled to go through a heating process, a heat preservation process, a primary cooling process, a secondary cooling process and a tertiary cooling process in sequence. During the annealing process, circulating hot air is used to heat the annealing furnace so that the air in the furnace circulates, thereby making the lens 3 heated more evenly;

[0046] S31 Heating process: Assuming the initial temperature is T0, the temperature is raised to the insulation temperature T1 at a rate of 2.5-4°C / min, and the preferred heating rate is 3-3.5°C / min. The heating rate in this step is K1, wherein T1=(Ta+Tstp) / 2, Ta is the annealing point temperature of the glass aspherical lens 3 material, and Tstp is the strain point temperature of the glass aspherical lens 3 material;

[0047] S32 insulation process: at the temperature T1, the glass aspheric lens 3 is heat-insulated and heated, and the insulation heating time is t, wherein the insulation time t=α·η·D+60, α is the heating coefficient (min / mm), η is the correction coefficient of the furnace loading condition; D is the maximum thickness of the aspheric lens 3 (mm), and the appropriate insulation time is set according to the maximum thickness of the glass lens 3 to eliminate thermal stress and restore the design value of the optical constant;

[0048] S33: first cooling process: cool down the temperature T1 to the temperature T2 at a rate of 0.3-0.7°C / min. The preferred cooling rate in the first cooling process is 0.4-0.5°C / min. The cooling rate in this step is K2, where T2=Tstp-100°C. During the first cooling process, the temperature of the lens 3 is relatively high. The slow cooling process can effectively prevent the lens 3 from generating new thermal stress.

[0049] S34 second cooling process: cool down the temperature T2 to the temperature T3 at a rate of 0.8-1.2°C / min. The preferred cooling rate in the second cooling process is 0.9-1.1°C / min. The cooling rate in this step is K3, where T3 = Tstp-200°C.

[0050] S35 third cooling process: cool down the temperature T3 to the temperature T4 at a rate of 1.3-2°C / min, preferably the cooling rate in the third cooling process is 1.4-1.5°C / min, the cooling rate in this step is K4, wherein the temperature of T4 is 50-100°C, preferably the temperature of T4 is 50-60°C;

[0051] S36 When the temperature reaches T4, the addition of inert gas is turned off, the heating of the annealing furnace is stopped, the furnace door is opened 1 / 3 of the way, and the annealing furnace is allowed to cool naturally to room temperature;

[0052] S4 Material inspection: open the furnace door, take out the glass aspheric lens 3, and inspect the residual thermal stress, aspheric surface error, refractive index, dispersion coefficient, center thickness, outer diameter and surface appearance of the glass aspheric lens 3. Specifically, use Talysurf PGI 1240 profilometer to inspect the surface shape of the glass aspheric lens 3, and the surface error must meet the requirements of the drawing; use a circular polarized light photoelastic stress measuring instrument to measure the residual thermal stress in the glass aspheric lens 3 before and after annealing; use an Abbe refractometer to measure the refractive index deviation and dispersion coefficient deviation in the lens before and after annealing, and the refractive index deviation is controlled within 0.03%, and the dispersion coefficient deviation is controlled within 0.06%; use a micrometer to measure the outer diameter of the glass aspheric lens 3 before and after annealing; use a thickness gauge to measure the center thickness of the glass aspheric lens 3 before and after annealing; use 40W white light to inspect the appearance of the surface of the glass aspheric lens 3.

[0053] The annealing method of this scheme is described below with reference to a specific embodiment.

[0054] Embodiment 1

[0055] Please refer to Figure 3 , and the following Table 1, the molded glass aspherical lens 3 of this embodiment uses a glass preform nitrate with a refractive index nd=1.69350 and an Abbe number vd=53.20, which is molded by a multi-axis molding device. The nitrate brand is HOYA's M-LAC130, and the glass nitrate parameter indicators are: strain point temperature Tstp=501°C, annealing point temperature Ta=520°C, and glass transition temperature Tg=525°C.

[0056]

[0057] In this embodiment, the surface equation of the aspheric surface is as follows:

[0058] Wherein, Z is the distance vector height from the vertex of the aspheric surface when the aspheric surface is at a height of r along the optical axis, c is the curvature of the aspheric surface at the paraxial direction, c=1 / R, R is the radius of curvature, k is the cone coefficient, A2 is the second-order coefficient of the aspheric surface, A4 is the fourth-order coefficient of the aspheric surface, A6 is the sixth-order coefficient of the aspheric surface, A8 is the eighth-order coefficient of the aspheric surface, A10 is the tenth-order coefficient of the aspheric surface, and A12 is the twelfth-order coefficient of the aspheric surface.

[0059] Table 1 below shows the surface parameters and dimensions of the aspheric lens.

[0060] Table 1: 3-surface parameters and dimensions of glass aspherical lenses

[0061]

[0062] The specific annealing steps are as follows

[0063] Please refer to Figure 4 S1 loading: Arrange and place the molded glass aspherical lenses 3 on the annealing tray 4, insert the annealing tray 4 into the hollow bracket 1, and then place the control price in the annealing furnace;

[0064] S2 ventilation: introducing an inert gas into the annealing furnace. In this embodiment, the introduced inert gas is nitrogen, and the introduced inert gas can also be argon, so that the volume proportion of oxygen in the annealing furnace is less than 0.8%. At the same time, the ventilation flow rate of the inert gas is controlled at 325 mL / min. The ventilation flow rate of the inert gas can also be controlled at 200 mL / min, 300 mL / min, 350 mL / min or 500 mL / min;

[0065] S3 annealing: the temperature is controlled to go through a heating process, a heat preservation process, a first cooling process, a second cooling process and a third cooling process in sequence. During the annealing process, circulating hot air is used to heat the annealing furnace.

[0066] S31 Heating process: Assume that the initial temperature is T0, and the temperature is raised to the insulation board temperature T1 at a rate of 3°C / min. The temperature can also be raised to the insulation board temperature T1 at a rate of 2.5°C / min, 3.5°C / min or 4°C / min; wherein T1 = (Ta + Tstp) / 2 = (501 + 520) / 2 = 510.5°C;

[0067] S32 heat preservation process: at the temperature T1, the glass aspherical lens 3 is heat-insulated and heated for a heat preservation and heating time of t, wherein the heat preservation time t=α·η·D+60, in this embodiment, α is 1.5min / mm, η is 1.2; D is 2.458mm, and the heat preservation time t is 64min after substitution and calculation;

[0068] S33 first cooling process: cooling the temperature from T1 to T2 at a rate of 0.5°C / min, or cooling the temperature from T1 to T2 at a rate of 0.3°C / min, 0.4°C / min or 0.7°C / min, wherein T2 = Tstp - 100°C = 401°C;

[0069] S34 second cooling process: cool down the temperature T2 to the temperature T3 at a rate of 1°C / min, and can also cool down the temperature T2 to the temperature T3 at a rate of 0.8°C / min, 0.9°C / min, 1.1°C / min or 1.2°C / min, wherein T3=Tstp-200°C=301°C;

[0070] S35: the third cooling process: cooling the temperature T3 to the temperature T4 at a rate of 1.5°C / min, or cooling the temperature T3 to the temperature T4 at a rate of 1.3°C / min, 1.4°C / min, or 2°C / min. In this embodiment, the temperature T4 is 50°C, or the temperature T4 can also be 60°C or 100°C.

[0071] S36 When the temperature reaches T4, the addition of inert gas is turned off, the heating of the annealing furnace is stopped, the furnace door is opened 1 / 3 of the way, and the annealing furnace is allowed to cool naturally to room temperature;

[0072] S4 Material removal inspection: open the furnace door, take out the glass aspherical lens 3, and inspect the glass aspherical lens 3.

[0073] After the present embodiment is treated by the annealing method disclosed in the present embodiment, the parameters of the lens 3 at different positions of the embodiment and the comparative example are tested using a Talysurf PGI 1240 profilometer, a circular polarized light photoelastic stress meter, an Abbe refractometer, a micrometer, a thickness gauge and 40W white light. The test results are shown in Table 2 below.

[0074] Table 2: Test results of Example 1

[0075]

[0076] Embodiment 2

[0077] Please refer to Figure 3 The structure of the molded glass aspheric lens 3 of this embodiment is the same as that of the glass aspheric lens 3 of the first embodiment, and the annealing method of the glass aspheric lens 3 of this embodiment is the same as that of the first embodiment. The difference is that in this embodiment, in step S2, the ventilation flow rate of the inert gas is controlled at 300 mL / min; in step S33, the first cooling rate K2 is 0.4°C / min; in step S34, the second cooling rate K3 is 0.9°C / min; in step S35, the third cooling rate K4 is 1.4°C / min.

[0078] After being treated by the annealing method disclosed in this embodiment, the parameters of the lens 3 at different positions of the embodiment and the comparative example were tested using a Talysurf PGI 1240 profilometer, a circularly polarized light photoelastic stress meter, an Abbe refractometer, a micrometer, a thickness gauge and 40W white light. The test results are shown in Table 3 below.

[0079] Table 3: Test results of Example 2

[0080]

[0081] Embodiment 3

[0082] Please refer to Figure 3 The structure of the molded glass aspheric lens 3 of this embodiment is the same as that of the glass aspheric lens 3 of the first embodiment, and the annealing method of the glass aspheric lens 3 of this embodiment is the same as that of the first embodiment. The difference is that in this embodiment, in step S2, the ventilation flow rate of the inert gas is controlled at 350 mL / min; in step S31, the heating rate K1 is 3.5°C / min; in step S34, the second cooling rate K3 is 1.1°C / min; in step S35, the third cooling rate K4 is 1.5°C / min.

[0083] After the present embodiment is treated by the annealing method disclosed in the present embodiment, the parameters of the lens 3 at different positions of the embodiment and the comparative example are tested using a Talysurf PGI 1240 profilometer, a circular polarized light photoelastic stress meter, an Abbe refractometer, a micrometer, a thickness gauge and 40W white light. The test results are shown in Table 4 below.

[0084] Table 4: Test results of Example 3

[0085]

[0086]

[0087] This solution also discloses the experimental results of Comparative Examples 1, 2 and 3:

[0088] The glass aspheric lens 3 before annealing in the comparative example 1 and the glass aspheric lens 3 before annealing in the present embodiment are obtained with the same parameters and are placed in the same annealing furnace as the present embodiment. The main difference is that in the comparative example, the glass aspheric lens 3 is placed on the annealing plate 2 and then directly on the annealing tray 4 in the annealing furnace, and the remaining annealing steps are the same as the annealing steps of the present embodiment.

[0089] The glass aspheric lens 3 before annealing in Comparative Example 2 and the glass aspheric lens 3 before annealing in this embodiment are obtained with the same parameters and are placed in the same annealing furnace as this embodiment. The main difference is that no inert gas is introduced into this comparative example, and annealing is performed directly in an oxygen environment. The remaining annealing steps are the same as the annealing steps of this embodiment.

[0090] The glass aspheric lens 3 before annealing in Comparative Example 3 and the glass aspheric lens 3 before annealing in this embodiment are obtained with the same parameters and are placed in the same annealing furnace as this embodiment. The main difference is that conventional annealing temperature and annealing heating rate and cooling rate are used, and the remaining annealing steps are the same as the annealing steps of this embodiment.

[0091] After the comparative example disclosed in this scheme is treated by the annealing method disclosed in this embodiment, the parameters of the lens 3 at different positions of the embodiment and the comparative example are tested using a Talysurf PGI 1240 profilometer, a circular polarized light photoelastic stress meter, an Abbe refractometer, a micrometer, a thickness gauge and 40W white light. The test results are shown in Table 4 below.

[0092] Table 4: Test results of Example 3

[0093]

[0094]

[0095] PV in Tables 2 to 4 is the aspheric surface error. It can be seen from Table 4 that in Comparative Example 1, the annealing plate 2 loaded with the glass aspheric lens 3 is directly placed in the annealing tray 4. Since the lower surface space of the glass aspheric lens 3 cannot be fully exchanged with the hot air, the annealing is insufficient. For example, the outer diameter and center thickness of the lens 1 in Comparative Example 1 are both over-specification, and the PV value of the lens 2 in Comparative Example 1 after annealing is over-specification, the refractive index deviates from the design value by as much as 0.258%, and the dispersion coefficient deviates from the design value by as much as 0.470%. This shows that the optical constants of the lens 3 after annealing have not been effectively restored, which has a great impact on the focusing and imaging quality of the lens 3.

[0096] In Comparative Example 2, the glass aspheric lens 3 is annealed in an oxygen environment. Since the unstable substances in the glass aspheric lens 3 react with oxygen, it is easy to cause the surface of the glass aspheric lens 3 to fog. As shown in the comparison, the surface fogging phenomenon of lens 1 and lens 2 is serious, and the refractive index and dispersion coefficient have a certain deviation from the design value, indicating that annealing in an inert gas environment can effectively prevent the occurrence of fogging on the lens surface.

[0097] Comparative Example 3 uses conventional annealing temperature and conventional heating temperature and cooling temperature for annealing. Due to the inaccurate control of heating temperature, and the heating rate and cooling rate being too fast or too slow, the aspheric surface shape error of the lens is large, the center thickness deviates far from the design value, and the average value of the center thermal stress decreases from 1.875Mpa before annealing to 0.240Mpa, with a decrease rate of only 87.20%. The refractive index deviates from the design value by as much as 0.208%, and the dispersion coefficient deviates from the design value by as much as 0.423%. It shows that the optical constants of lens 3 after annealing have not been effectively restored, which has a great impact on the focus and imaging quality of lens 3, indicating that the temperature setting values ​​of the heating temperature, heating rate, cooling rate, etc. of this scheme are more scientific and have better annealing effect.

[0098] In the first embodiment, the annealing plate 2 is loaded on a hollow annealing rack. The parameters of the lens 1 of the first embodiment, the lens 2 of the second embodiment and the lens 3 of the third embodiment are slightly different, indicating that the lens 3 is heated evenly and has good consistency through the improvement of the present invention.

[0099] The average PV values ​​of the A1 and A2 surfaces of the three lenses of Example 1 decreased from 0.970 μm and 0.465 μm before annealing to 0.183 μm and 0.125 μm respectively, and the surface shape error was greatly improved and met the design requirements of the lens 3. The central thermal stress of the three lenses 3 of Example 1 was measured using a circular polarized light photoelastic stress measuring instrument. The average central thermal stress decreased from 1.853 MPa before annealing to 0.03 MPa, with a decrease rate of 98.38%, indicating that the thermal stress was fully released and eliminated. The Nd (refractive index) and Vd (dispersion coefficient) were detected by Abbe refractometer. After annealing, the average Nd (refractive index) recovered from 1.68649 before annealing to 1.69317, which was only 0.019% different from the designed value of 1.6935. The Vd (dispersion coefficient) after annealing recovered from 52.78 before annealing to 53.18, which was only 0.044% different from the designed value of 53.20. This shows that the optical constants are well recovered after the annealing method of the present invention, close to the designed values, and have a good annealing effect.

[0100] The average PV values ​​of the A1 and A2 surfaces of the two lenses of Example 2 were reduced from 0.978 μm and 0.475 μm before annealing to 0.181 μm and 0.125 μm respectively, and the surface shape error was greatly improved and met the design requirements of the lens 3. The central thermal stress of the two lenses 3 of Example 2 was measured using a circular polarized light photoelastic stress measuring instrument. The average value of the central thermal stress was reduced from 1.815 MPa before annealing to 0.03 MPa, and the reduction rate also reached 98.35%, indicating that the thermal stress was fully released and eliminated. The Nd (refractive index) and Vd (dispersion coefficient) were detected by Abbe refractometer. After annealing, the average Nd (refractive index) recovered from 1.68691 before annealing to 1.69323, which was only 0.016% different from the designed value of 1.69350. The Vd (dispersion coefficient) after annealing recovered from 52.79 before annealing to 53.18, which was only 0.047% different from the designed value of 53.20. This shows that the optical constants are well recovered after the annealing method of the present invention, close to the designed values, and have a good annealing effect.

[0101] The average PV values ​​of the A1 and A2 surfaces of the two lenses of Example 3 decreased from 0.970 μm and 0.471 μm before annealing to 0.183 μm and 0.126 μm respectively, and the surface shape error was greatly improved and met the design requirements of the lens 3. The central thermal stress of the two lenses 3 of Example 3 was measured using a circular polarized light photoelastic stress measuring instrument. The average value of the central thermal stress decreased from 1.855 MPa before annealing to 0.03 MPa, and the decrease rate also reached 98.38%, indicating that the thermal stress was fully released and eliminated. The Nd (refractive index) and Vd (dispersion coefficient) were detected by Abbe refractometer. After annealing, the average Nd (refractive index) recovered from 1.68631 before annealing to 1.69321, which was only 0.017% different from the designed value of 1.69350. The Vd (dispersion coefficient) after annealing recovered from 52.77 before annealing to 53.17, which was only 0.056% different from the designed value of 53.20. This shows that the optical constants are well recovered after the annealing method of the present invention, close to the designed values, and have a good annealing effect.

[0102] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0103] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for annealing a glass aspherical lens, characterized in that: The steps include: S1 Loading: Arrange the molded lenses on the hollow bracket, place the hollow bracket in the annealing furnace, and close the furnace door; S2 ventilation: Inert gas is introduced into the annealing furnace so that the volume proportion of oxygen in the annealing furnace is less than 0.8%; S3 annealing: the temperature is controlled to go through a heating process, a heat preservation process, a first cooling process, a second cooling process and a third cooling process in sequence; S31: the heating process is as follows: assuming the initial temperature to be T0, heating to the holding temperature T1 at a rate of 2.5-4°C / min; S32: the heat preservation process: heat the glass aspherical lens at a temperature of T1 for a heat preservation time of t; The first cooling process in S33: cooling the temperature T1 to the temperature T2 at a rate of 0.3-0.7°C / min; S34: the secondary cooling process: cooling the temperature from T2 to T3 at a rate of 0.8-1.2°C / min; S35: cooling down the temperature from T3 to T4 at a rate of 1.3-2°C / min; S4 Material inspection: Open the furnace door, take out the glass aspheric lens, and inspect the residual thermal stress, aspheric surface error, refractive index, dispersion coefficient, center thickness, outer diameter and surface appearance of the glass aspheric lens.

2. The annealing method of a glass aspherical lens according to claim 1, characterized in that: In step S2, the inert gas is nitrogen or argon.

3. The annealing method of a glass aspherical lens according to claim 1, characterized in that: In step S2, the ventilation flow rate of the inert gas is greater than 200 mL / min.

4. The annealing method of a glass aspherical lens according to claim 1, characterized in that: In step S31, T1=(Ta+Tstp) / 2, Ta is the annealing point temperature of the glass aspherical lens material, and Tstp is the strain point temperature of the glass aspherical lens material.

5. The annealing method of a glass aspherical lens according to claim 4, characterized in that: In step S33, T2=Tstp-100°C.

6. The annealing method of a glass aspherical lens according to claim 4, characterized in that: In step S34, T3 = Tstp - 200°C.

7. The annealing method of a glass aspherical lens according to claim 4, characterized in that: In step S35, the temperature of T4 is 50-100°C.

8. The annealing method of a glass aspherical lens according to claim 1, characterized in that: In step S3, the annealing furnace is heated by circulating hot air during the annealing process.

9. The annealing method of a glass aspherical lens according to claim 1, characterized in that: The method further includes step S36, when the temperature reaches T4, closing the addition of the inert gas, stopping heating the annealing furnace, opening the furnace door 1 / 3 of the way, and allowing the annealing furnace to cool naturally to room temperature.

10. The annealing method of a glass aspherical lens according to claim 1, characterized in that: In step S32, the holding time t=α·η·D+60, wherein α is the heating coefficient, in units of min / mm, η is the correction coefficient of the furnace loading condition; and D is the maximum thickness of the aspherical lens, in units of mm.

Citation Information

Patent Citations

  • Forming method of chalcogenide glass aspherical lens

    CN104310755A

  • Optical lens and manufacturing method

    CN110256640A

  • Glass precision compression molding method and device

    CN110903021A

  • Annealing method of sapphire glass panel

    CN113718339A

  • Atmosphere protection precision annealing furnace for optical glass aspheric lens

    CN113912274A