A method for separating metal elements from waste nickel-hydrogen batteries

Through the combination of oxidative roasting and acid leaching processes, the problem of difficulty in separation of rare earth elements and transition metal elements in waste nickel-hydrogen batteries is solved, and efficient metal element recycling is achieved, which improves the recovery rate and reduces the environmental pressure.

CN115852149BActive Publication Date: 2024-11-01GANJIANG INNOVATION ACAD CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211642470.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-20
Publication Date
2024-11-01
Estimated Expiration
2042-12-20

AI Technical Summary

Technical Problem

In the prior art, it is difficult to selectively separate rare earth elements from transition metals in waste nickel-hydrogen batteries, resulting in low metal recovery and large chemical consumption, which increases environmental pressure.

Method used

Using a combination of oxidative roasting and acid leaching processes, combining specific additives with oxidative roasting, different leaching processes are used to achieve step-by-step selective leaching of rare earth elements and transition metal elements, and the rare earth sulfate solution with higher purity is separated and Transition metal sulfate solution.

Benefits of technology

The efficient recycling of rare earth elements and transition metal elements in waste nickel-hydrogen batteries is achieved, with the rare earth element recovery rate ≥95%, and the transition metal element recovery rate ≥97%, reducing chemical consumption and environmental pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115852149B_ABST
    Figure CN115852149B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for separating metal elements from waste nickel-hydrogen batteries, the separation method comprising the following steps: (1) ball-milling waste nickel-hydrogen battery powder and sulfate and then oxidizing and roasting to obtain a roasted product; (2) water-leaching the product obtained in step (1) to obtain rare earth leaching solution and leaching residue through solid-liquid separation; (3) acid-leaching the leaching residue obtained in step (2) to obtain transition metal element leaching solution through solid-liquid separation. The separation method provided by the present invention combines specific additives with oxidizing and roasting, and utilizes different leaching processes to couple to achieve step-by-step selective leaching of rare earth elements and transition metal elements, thereby achieving step-by-step efficient recovery of metal elements from waste nickel-hydrogen batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resource recycling, and in particular to a method for separating metal elements in waste nickel-hydrogen batteries. Background Art

[0002] At present, the transformation of energy structure and renewable energy have increased the demand for energy storage in the power system. NiMH batteries do not contain heavy metals such as cadmium, are green and environmentally friendly, have a long life, high specific capacity, low self-discharge rate, a wide operating temperature range (-20~50℃), and are highly safe. Therefore, they are widely used in wireless communications, portable electronic devices, hybrid batteries, and electrochemical energy storage. The service life of NiMH batteries is 2-3 years. The recycling of each set of NiMH batteries will save about 83kg of CO 2 Emissions, 1.37kg of resource consumption, 0.044m 3 The amount of landfill and energy consumption of 1611MJ. The waste NiMH positive electrode materials of HEV mainly contain about 70wt% Ni, 6wt% Co, and 1wt% REE; the negative electrode materials contain 52wt% Ni, 5wt% Mn, 4wt% Co, 1.7wt% Al, 32wt% REE and other valuable metals. If they can be effectively recycled, it can not only alleviate the metal resource crisis in my country, but also reduce the environmental pollution risk caused by these metals.

[0003] The existing methods for recycling waste nickel-hydrogen batteries mainly include physical pretreatment, pyrolysis and wet processing.

[0004] For example, CN106935923A discloses a method for recovering valuable metals from waste nickel-hydrogen batteries, which comprises the following steps: (1) analyzing the physical structure and chemical composition of waste nickel-hydrogen batteries to clarify the composition of the batteries and the content and existence form of each metal element in each part of the batteries; (2) disassembling and crushing the waste nickel-hydrogen batteries and then screening them to separate the current collector from the active material, and using a vacuum distillation process to recover the high vapor pressure and low melting point metals in the waste nickel-hydrogen batteries; (3) using a magnetic separation process to recover the residues of the waste nickel-hydrogen batteries after vacuum distillation. This scheme uses a pressurized hydrometallurgical method, assisted by mechanical physics, magnetic separation and other methods to study the process for recovering valuable metals in waste nickel-hydrogen batteries, and utilizes the characteristics of the pressurized hydrometallurgical process technology that is suitable for processing complex and difficult-to-select non-ferrous metal resources to achieve comprehensive utilization of resources.

[0005] CN101886178A discloses a comprehensive recycling method for nickel-hydrogen waste batteries, including crushing the nickel-hydrogen waste batteries, magnetic separation and screening; preparing a leachate containing sulfuric acid and an oxidant; putting the powder under the sieve into the leachate, heating it to 50-100°C, and leaching for 1-3 hours; solid-liquid separation, adjusting the pH value of the filtrate to 2-5, adding a water-soluble sulfate, and precipitating the rare earth elements therein; solid-liquid separation, adding an extractant to the filtrate to remove impurities, and obtaining a sulfate solution containing nickel and cobalt. The nickel-hydrogen waste battery recycling method of this scheme can effectively recover various valuable metal elements in various nickel-hydrogen batteries. The sulfate solution containing nickel and cobalt after extraction and purification can be directly used in the production of spherical nickel hydroxide, the positive electrode material of nickel-hydrogen batteries. Less energy is consumed in the recycling process, the recycling process route is short, and the recycling efficiency is good.

[0006] However, in the existing recycling methods, waste nickel-hydrogen batteries usually need to be pre-processed by physical methods such as disassembly, grinding, and screening to facilitate subsequent recycling. The pyrometallurgical method has high adaptability to raw materials from different sources and a large processing capacity, but it is difficult to achieve selective separation of metal elements. The result is Ni-Co alloy, while rare earth elements are retained in the slag and lost. The wet process usually uses acid leaching, and the resulting mixed metal salt solution needs to be further separated through multi-step chemical precipitation, solvent extraction and other methods. The recycling process is redundant, the metal recovery rate is low, and the chemical consumption is large. The waste generated needs to be further processed and the energy consumption is high, which increases the pressure on the environment. Summary of the invention

[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for separating metal elements in waste nickel-hydrogen batteries to solve the technical difficulties existing in the prior art, such as the difficulty in separating transition metals and rare earth elements in the leaching process and the low metal recovery rate.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for separating metal elements in waste nickel-hydrogen batteries, the separation method comprising the following steps:

[0010] (1) ball-milling waste nickel-hydrogen battery powder and sulfate, followed by oxidative roasting to obtain a roasted product;

[0011] (2) subjecting the product obtained in step (1) to water leaching, and obtaining rare earth leaching solution and leaching residue by solid-liquid separation;

[0012] (3) The leached residue obtained in step (2) is subjected to acid leaching, and a transition metal element leaching solution is obtained through solid-liquid separation.

[0013] The separation method provided by the present invention combines specific additives with oxidative roasting and utilizes different leaching processes to couple to achieve step-by-step selective leaching of rare earth elements and transition metal elements, thereby achieving step-by-step and efficient recovery of metal elements in waste nickel-hydrogen batteries.

[0014] In the present invention, the particle size of the waste nickel-hydrogen battery is less than 106 μm, and it can be a particle aggregate within a certain particle size range, such as a cluster of particles within a particle size range of 20-80 μm, a cluster of particles within a range of 10-50 μm, a cluster of particles within a range of 50-100 μm, or a cluster of particles smaller than a certain particle size, such as all particle clusters within a range of ≤80 μm, all particle clusters within a range of ≤60 μm, all particle clusters within a range of ≤20 μm, etc.

[0015] As a preferred technical solution of the present invention, the sulfate in step (1) includes one or a combination of at least two of nickel sulfate, cobalt sulfate, manganese sulfate, aluminum sulfate, iron sulfate or ammonium sulfate. The sulfate used reacts with the rare earth elements in the nickel-hydrogen battery powder under oxidative roasting conditions to convert the rare earth elements into rare earth metal sulfates, while the transition metal elements are converted into metal oxides under the same conditions. Taking ammonium sulfate as an example, the reaction equation is as follows:

[0016] 3(NH 4 ) 2 SO 4 +2LaNi 5 +6.5O 2 =10NiO+La 2 (SO 4 ) 3 +6NH 3 +3H 2 O

[0017] Preferably, the amount of sulfate added in step (1) is n( ):n(RE)=(0.9-2):1, for example, it can be 0.9:1, 0.95:1, 1:1, 1.05:1, 1.1:1, 1.15:1, 1.2:1, 1.25:1, 1.3:1, 1.35:1, 1.4:1, 1.45:1, 1.5:1, 1.55:1, 1.6:1, 1.65:1, 1.7:1, 1.75:1, 1.8:1, 1.85:1, 1.9:1, 1.95:1 or 2:1, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0018] Preferably, the rotation speed of the ball milling treatment in step (1) is 300-600 r / min, for example, it can be 300 r / min, 320 r / min, 340 r / min, 360 r / min, 380 r / min, 400 r / min, 420 r / min, 440 r / min, 460 r / min, 480 r / min, 500 r / min, 520 r / min, 540 r / min, 560 r / min, 580 r / min or 600 r / min, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0019] Preferably, the mass ratio of ball milling medium to powder in the ball milling treatment in step (1) is (5-30):1, for example, it can be 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1, 5:1,

[0020] Preferably, the ball milling time in step (1) is 15-120 min, for example, it can be 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, 90 min, 95 min, 100 min, 105 min, 110 min, 115 min or 120 min, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0021] As a preferred technical solution of the present invention, the volume content of the gaseous oxidant in the atmosphere used in the oxidative roasting in step (1) is greater than 20%, for example, it can be 22%, 24%, 26%, 28%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or 100%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0022] In the present invention, the gas oxidant may be oxygen and / or ozone, and the volume concentration may be adjusted by using an inert gas such as carbon dioxide or nitrogen.

[0023] As a preferred technical solution of the present invention, the temperature of the oxidative roasting in step (1) is 900-1200°C, for example, it can be 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, 1020°C, 1040°C, 1060°C, 1080°C, 1100°C, 1120°C, 1140°C, 1160°C, 1180°C or 1200°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0024] Preferably, the oxidative roasting time in step (1) is 30-120 min, for example, it can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, 90 min, 95 min, 100 min, 105 min, 110 min, 115 min or 120 min, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0025] As a preferred technical solution of the present invention, the liquid-to-solid ratio of the water immersion in step (2) is (3-10):1 in mL / g, for example, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1 or 10:1, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0026] As a preferred technical solution of the present invention, the water immersion temperature in step (2) is 25-80°C, for example, it can be 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0027] Preferably, the immersion time in step (2) is 30-120 min, for example, it can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, 90 min, 95 min, 100 min, 105 min, 110 min, 115 min or 120 min, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0028] As a preferred technical solution of the present invention, the acid used in the acid leaching in step (3) includes one or a combination of at least two of sulfuric acid, nitric acid or hydrochloric acid.

[0029] Preferably, the concentration of the acid used in the acid leaching in step (3) is 0.5-3 mol / L, for example, it can be 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L, 2 mol / L, 2.1 mol / L, 2.2 mol / L, 2.3 mol / L, 2.4 mol / L, 2.5 mol / L, 2.6 mol / L, 2.7 mol / L, 2.8 mol / L, 2.9 mol / L or 3 mol / L, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0030] As a preferred technical solution of the present invention, the liquid-to-solid ratio of the acid leaching in step (3) is (3-10):1, for example, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1 or 10:1, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0031] As a preferred technical solution of the present invention, the temperature of the acid leaching in step (3) is 25-80°C, for example, it can be 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0032] Preferably, the acid leaching time in step (3) is 30-240 min, for example, it can be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 210 min, 220 min, 230 min or 240 min, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0033] As a preferred technical solution of the present invention, the separation method comprises the following steps:

[0034] (1) After ball-milling waste nickel-hydrogen battery powder and sulfate, oxidative roasting is performed to obtain a roasted product; the sulfate comprises one or a combination of at least two of nickel sulfate, cobalt sulfate, manganese sulfate, aluminum sulfate, iron sulfate or ammonium sulfate; the amount of the sulfate added is n( ):n(RE)=(0.9-2):1; the rotation speed of the ball milling treatment is 300-600r / min; the mass ratio of the ball milling medium to the powder in the ball milling treatment is (5-30):1; the time of the ball milling treatment is 15-120min; the volume content of the gas oxidant in the atmosphere used in the oxidation roasting is greater than 20%; the temperature of the oxidation roasting is 900-1200℃; the time of the oxidation roasting is 30-120min;

[0035] (2) subjecting the product obtained in step (1) to water leaching, and obtaining rare earth leaching solution and leaching residue by solid-liquid separation; the liquid-solid ratio of the water leaching is (3-10):1; the water leaching temperature is 25-80°C; and the water leaching time is 30-120min;

[0036] (3) subjecting the leached residue obtained in step (2) to acid leaching, and obtaining a transition metal element leaching solution through solid-liquid separation; the acid used in the acid leaching comprises one or a combination of at least two of sulfuric acid, nitric acid or hydrochloric acid; the concentration of the acid used in the acid leaching is 0.5-3 mol / L; the liquid-to-solid ratio of the acid leaching is (3-10):1 in mL / g; the temperature of the acid leaching is 25-80°C; and the time of the acid leaching is 30-240 min.

[0037] Compared with the prior art solutions, the present invention has the following beneficial effects:

[0038] (1) The oxidation roasting and acid leaching process provided by the present invention can solve the disadvantage of the existing nickel-hydrogen battery powder leaching process that rare earth metal elements and transition metal elements are difficult to separate. The purpose of step-by-step selective leaching of rare earth metal elements and transition metal elements is achieved by coupling the oxidation roasting, water leaching and acid leaching processes, and a rare earth sulfate solution and a transition metal sulfate solution with high purity are obtained.

[0039] (2) The separation method provided by the present invention realizes the separation of rare earth elements and transition metal elements in waste nickel-hydrogen batteries. The recovery rate of rare earth elements is ≥95%, the recovery rate of transition metal elements is ≥97%, the leaching rate of rare earth elements in water leaching is ≥95%, and the leaching rate of transition metal elements in acid leaching is ≥97%. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 The present invention is a flowchart of a method for separating metal elements from waste nickel-hydrogen batteries.

[0041] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION

[0042] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0043] like Figure 1 As shown, waste nickel-hydrogen battery powder is ball-milled with sulfate and then oxidized and roasted to obtain a roasted product; the roasted product is mixed with water and leached, and the solid and liquid are separated after leaching to obtain a rare earth leaching solution and a leaching residue; the leaching residue is leached with acid, and the solid and liquid are separated after leaching to obtain a transition metal leaching solution.

[0044] Example 1

[0045] This embodiment provides a method for separating metal elements in waste nickel-hydrogen batteries, which is as follows:

[0046] (1) Grinding the waste nickel-hydrogen battery electrode material with an agate mortar and passing it through a 150-mesh sieve, and drying it at 80° C. overnight to obtain a powder 1;

[0047] (2) Powder 1 and ammonium sulfate are mixed at a molar ratio of n( ):n(RE)=1:1 after ball milling (rotation speed 300r / min, ball-to-material ratio 5:1, time 60min), calcined at 900℃ (calcination atmosphere is ozone) for 60min to obtain powder 2;

[0048] (3) Mixing powder 2 with water at a liquid-to-solid ratio of 5:1, leaching at 60°C for 90 min, separating the solid and liquid to obtain rare earth leaching solution and leaching residue, and drying to obtain powder 3;

[0049] (4) The powder 3 was leached with 0.5 mol / L nitric acid at a liquid-solid ratio of 5:1 at 60°C for 60 min. After leaching, the solid and liquid were separated to obtain a transition metal leachate and a leaching residue.

[0050] In this embodiment, the total recovery rate of rare earth elements in step (3) was calculated to be 96.19%, the nickel leaching rate was 1.35%, the cobalt leaching rate was 1.98%, and the zinc leaching rate was 0.67% by inductively coupled plasma optical emission spectroscopy (ICP-OES). According to X-ray diffraction (XRD) analysis, the main phase of the solid slag in step (3) was transition metal oxide. The nickel recovery rate in step (4) was calculated to be 99.49%, the cobalt recovery rate was 98.62%, and the zinc recovery rate was 99.73%.

[0051] Example 2

[0052] This embodiment provides a method for separating metal elements in waste nickel-hydrogen batteries, which is as follows:

[0053] (1) Grinding the waste nickel-hydrogen battery electrode material with an agate mortar and passing it through a 150-mesh sieve, and drying it at 80° C. overnight to obtain a powder 1;

[0054] (2) Powder 1 and nickel sulfate are mixed at a molar ratio of n( ):n(RE)=2:1 After ball milling (rotation speed 600r / min, ball-to-material ratio 30:1, time 120min), calcination at 1200℃ (calcination atmosphere is oxygen) for 90min to obtain powder 2;

[0055] (3) Mixing powder 2 with water at a liquid-to-solid ratio of 10:1, leaching at 70°C for 120 min, separating the solid and liquid to obtain rare earth leaching solution and leaching residue, and drying to obtain powder 3;

[0056] (4) The powder 3 was leached with 1 mol / L nitric acid at a liquid-to-solid ratio of 10:1 at 70°C for 120 min. After leaching, the solid and liquid were separated to obtain a transition metal leaching solution and a leaching residue.

[0057] In this embodiment, the total recovery rate of rare earth elements in step (3) was calculated to be 99.81%, the nickel leaching rate was 0.97%, the cobalt leaching rate was 1.20%, and the zinc leaching rate was 0.58% by inductively coupled plasma optical emission spectroscopy (ICP-OES). According to X-ray diffraction (XRD) analysis, the main phase of the solid slag in step (3) was transition metal oxide. The nickel recovery rate in step (4) was calculated to be 98.13%, the cobalt recovery rate was 98.82%, and the zinc recovery rate was 98.39%.

[0058] Comparative Example 1

[0059] The only difference from Example 1 is that step (2) and step (4) are not performed, and step (3) and subsequent testing and data processing are performed directly after step (1).

[0060] Through inductively coupled plasma optical emission spectroscopy (ICP-OES) detection, it was calculated that the total recovery rate of rare earth elements in water leaching was 0.54%, the nickel recovery rate was 0.13%, the cobalt recovery rate was 0.03%, and the zinc recovery rate was 0.04%.

[0061] Comparative Example 2

[0062] The only difference from Example 1 is that steps (2) and (3) are not performed, and steps (1) and (4) are performed directly.

[0063] According to inductively coupled plasma optical emission spectroscopy (ICP-OES) detection, the total recovery rate of rare earth elements in acid leaching was calculated to be 54%, the nickel recovery rate was 89.78%, the cobalt recovery rate was 87.60%, and the zinc recovery rate was 85.54%.

[0064] Comparative Example 3

[0065] The only difference from Example 1 is that ammonium sulfate is replaced by an equal amount of sulfuric acid.

[0066] According to inductively coupled plasma optical emission spectroscopy (ICP-OES) detection, the total recovery rate of rare earth elements in step (3) was calculated to be 60.81%, the nickel leaching rate was 50.97%, the cobalt leaching rate was 51.20%, and the zinc leaching rate was 40.58%. According to X-ray diffraction (XRD) analysis, the main phases of the solid slag in step (3) were transition metal oxides and rare earth oxides. The nickel recovery rate in step (4) was calculated to be 98.13%, the cobalt recovery rate was 98.82%, the zinc recovery rate was 98.39%, and the leaching rate of rare earth elements was 90.51%.

[0067] Comparative Example 4

[0068] The only difference from Example 1 is that the calcination temperature is adjusted to 500°C.

[0069] According to the inductively coupled plasma optical emission spectroscopy (ICP-OES) detection, the total recovery rate of rare earth elements in water leaching was calculated to be 86.57%, the nickel leaching rate was 52.13%, the cobalt leaching rate was 42.57%, and the zinc leaching rate was 51.65%. According to X-ray diffraction (XRD) analysis, the main phases of the solid slag obtained after water leaching were transition metal hydroxides and rare earth metal hydrides. After acid leaching, the nickel recovery rate was 93.46%, the cobalt recovery rate was 89.01%, the zinc recovery rate was 90.06%, and the recovery rate of rare earth elements was 92.54%.

[0070] Comparative Example 5

[0071] The only difference from Example 1 is that the calcination is carried out under a nitrogen atmosphere.

[0072] According to the inductively coupled plasma optical emission spectroscopy (ICP-OES) detection, the total recovery rate of rare earth elements in water leaching was calculated to be 42.80%, the nickel leaching rate was 62.28%, the cobalt leaching rate was 52.89%, and the zinc leaching rate was 61.71%. According to X-ray diffraction (XRD) analysis, the main phases of the solid slag obtained after water leaching were transition metal elements and rare earth metal elements. After acid leaching, the nickel recovery rate was 92.25%, the cobalt recovery rate was 85.14%, the zinc recovery rate was 86.12%, and the rare earth element recovery rate was 95.68%.

[0073] Comparative Example 6

[0074] The only difference from Example 1 is that the ball milling process is replaced by conventional stirring and mixing.

[0075] According to the inductively coupled plasma optical emission spectroscopy (ICP-OES) detection, the total recovery rate of rare earth elements in water leaching was calculated to be 77.12%, the nickel leaching rate was 3.28%, the cobalt leaching rate was 2.26%, and the zinc leaching rate was 3.17%. According to X-ray diffraction (XRD) analysis, the main phases of the solid slag obtained after water leaching were transition metal hydroxides and rare earth metal hydrides. After acid leaching, the nickel recovery rate was 92.47%, the cobalt recovery rate was 85.27%, and the zinc recovery rate was 86.25%.

[0076] Comparative Example 7

[0077] The only difference from Example 1 is that ammonium sulfate is replaced by an equal amount of ferrous disulfide.

[0078] According to the inductively coupled plasma optical emission spectroscopy (ICP-OES) detection, the total recovery rate of rare earth elements in water leaching was calculated to be 55.63%, the nickel leaching rate was 3.47%, the cobalt leaching rate was 2.17%, and the zinc leaching rate was 3.56%. According to X-ray diffraction (XRD) analysis, the main phases of the solid slag obtained after water leaching were transition metal hydroxides and rare earth metal hydrides. After acid leaching, the nickel recovery rate was 91.45%, the cobalt recovery rate was 89.60%, the zinc recovery rate was 83.65%, and the rare earth element leaching rate was 87.34%.

[0079] Comparative Example 8

[0080] The only difference from Example 1 is that the rotation speed in the ball milling process is adjusted to 100 r / min.

[0081] According to the inductively coupled plasma optical emission spectroscopy (ICP-OES) detection, the total recovery rate of rare earth elements in water leaching was calculated to be 87.57%, the nickel leaching rate was 2.79%, the cobalt leaching rate was 2.09%, and the zinc leaching rate was 2.26%. According to X-ray diffraction (XRD) analysis, the main phases of the solid slag obtained after water leaching were transition metal hydroxides and rare earth metal hydrides. After acid leaching, the nickel recovery rate was 90.47%, the cobalt recovery rate was 89.35%, and the zinc recovery rate was 84.23%.

[0082] It can be seen from the above embodiments and comparative examples that by combining high-speed ball milling and sulfate treatment, rare earth elements are converted into water-soluble rare earth sulfates, while transition metals are converted into metal oxides, thereby achieving separation of rare earth elements and transition metal elements through water leaching.

[0083] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0084] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0085] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0086] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for separating metal elements from waste nickel-hydrogen batteries. It is characterized in that The separation method comprises the following steps: (1) ball-milling waste nickel-hydrogen battery powder and sulfate and then oxidizing and roasting them to obtain a roasted product; The volume content of the gaseous oxidant in the atmosphere used in the oxidation roasting is greater than 20%; The rotation speed of the ball milling process is 300-600r / min; The sulfate includes one or a combination of at least two of nickel sulfate, cobalt sulfate, manganese sulfate, aluminum sulfate, iron sulfate or ammonium sulfate; (2) subjecting the product obtained in step (1) to water leaching, and obtaining rare earth leaching solution and leaching residue by solid-liquid separation; (3) The leached residue obtained in step (2) is subjected to acid leaching, and a transition metal element leaching solution is obtained through solid-liquid separation.

2. The separation method according to claim 1, It is characterized in that The amount of sulfate added in step (1) is n( ):n(RE)=(0.9-2):

1.

3. The separation method according to claim 1, It is characterized in that In the ball milling process of step (1), the mass ratio of the ball milling medium to the powder is (5-30):

1.

4. The separation method according to claim 1, It is characterized in that The ball milling time in step (1) is 15-120 minutes.

5. The separation method according to claim 1, It is characterized in that The temperature of the oxidation roasting in step (1) is 900-1200°C.

6. The separation method according to claim 1, It is characterized in that The time of the oxidative roasting in step (1) is 30-120 minutes.

7. The separation method according to claim 1, It is characterized in that The liquid-to-solid ratio of the water immersion in step (2) is (3-10):

1.

8. The separation method according to claim 1, It is characterized in that The water immersion temperature in step (2) is 25-80°C.

9. The separation method according to claim 1, It is characterized in that The immersion time in step (2) is 30-120 minutes.

10. The separation method according to claim 1, It is characterized in that The acid used in the acid leaching in step (3) includes one or a combination of at least two of sulfuric acid, nitric acid or hydrochloric acid.

11. The separation method according to claim 1, It is characterized in that The concentration of the acid used in the acid leaching in step (3) is 0.5-3 mol / L.

12. The separation method according to claim 1, It is characterized in that The liquid-to-solid ratio of the acid leaching in step (3) is (3-10):1 in mL / g.

13. The separation method according to claim 1, It is characterized in that The acid leaching temperature in step (3) is 25-80°C.

14. The separation method according to claim 1, It is characterized in that The acid leaching time in step (3) is 30-240 minutes.

15. The separation method according to claim 1, It is characterized in that The separation method comprises the following steps: (1) After ball-milling waste nickel-hydrogen battery powder and sulfate, oxidative roasting is performed to obtain a roasted product; the sulfate comprises one or a combination of at least two of nickel sulfate, cobalt sulfate, manganese sulfate, aluminum sulfate, iron sulfate or ammonium sulfate; the amount of the sulfate added is n( ):n(RE)=(0.9-2):1; the rotation speed of the ball milling treatment is 300-600r / min; the mass ratio of the ball milling medium to the powder in the ball milling treatment is (5-30):1; the time of the ball milling treatment is 15-120min; the volume content of the gas oxidant in the atmosphere used in the oxidation roasting is greater than 20%; the temperature of the oxidation roasting is 900-1200℃; the time of the oxidation roasting is 30-120min; (2) subjecting the product obtained in step (1) to water leaching, and obtaining rare earth leaching solution and leaching residue by solid-liquid separation; the liquid-solid ratio of the water leaching is (3-10):1; the water leaching temperature is 25-80°C; and the water leaching time is 30-120min; (3) subjecting the leached residue obtained in step (2) to acid leaching, and obtaining a transition metal element leaching solution through solid-liquid separation; the acid used in the acid leaching comprises one or a combination of at least two of sulfuric acid, nitric acid or hydrochloric acid; the concentration of the acid used in the acid leaching is 0.5-3 mol / L; the liquid-to-solid ratio of the acid leaching is (3-10):1 in mL / g; the temperature of the acid leaching is 25-80°C; and the time of the acid leaching is 30-240 min.