Processing method of anti-ultraviolet lyocell fabric

By designing the weft pattern ratio in lyocell fabrics, performing alkali treatment and mechanical polishing, and fixing anti-UV additives, the problem of poor anti-UV effect of ultra-light fabrics has been solved, significantly improving the UPF value and maintaining excellent UV resistance.

CN115852677BActive Publication Date: 2024-10-18LU FENG WEAVING & DYEING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211585286.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-18
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The plain ultra-light lyocell fabric with a warp and weft count of 120s, a warp density of 200 threads/inch, and a weft density of 150 threads/inch has poor UV resistance, which limits its use.

Method used

Through tissue specification design, the weft pattern ratio of lyocell to polyester is set to 3:1, followed by mild alkali treatment and mechanical polishing, and then a benzotriazole compound containing acryloyl groups is fixed on the fabric to improve the fabric's UV resistance. performance.

Benefits of technology

The UPF value has been increased from untreated 15 to over 50, and the UV resistance is long-lasting. The UPF value can still reach over 50 after 30 times of washing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003990680780000041
    Figure BDA0003990680780000041
Patent Text Reader

Abstract

The present invention belongs to the technical field of textile printing and dyeing, and specifically relates to a method for processing UV-resistant lyocell fabrics. The UV-resistant lyocell fabric processing method comprises a fabric finishing process flow of: alkali treatment → mechanical polishing → fixation treatment. The method achieves a huge improvement in UPF value from 15 before treatment to more than 50 through organization specification design, mild alkali treatment, and fixation of acryl-containing benzotriazole compounds on the lyocell fabric after mechanical polishing, and has durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile printing and dyeing, and particularly relates to a processing method of anti-ultraviolet lyocell fabric. Background Art

[0002] Lyocell fiber is an important member of the renewable fiber. The fabrics made from it are soft, light, lively and very suitable for women's clothing fabrics. They are highly sought after by consumers. Lyocell fiber has excellent mechanical properties, the comfort of cotton fiber and the strength of polyester. It is not only a green fiber with renewable raw materials, but also biodegradable after use.

[0003] However, this type of fabric is used for light outerwear, and has poor UV protection, which limits the scope of use. During production, it was found that the plain ultra-light Lyocell fabric with warp and weft yarn counts of 120s, warp yarn density of 200 yarns / inch, and weft yarn density of 150 yarns / inch has poor UV protection. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a processing method for UV-resistant lyocell fabric. Through organizational specification design, mild alkali treatment and fixation of acryl-containing benzotriazole compounds on the lyocell fabric after mechanical polishing, the UPF value is greatly improved from 15 of untreated to more than 50. The process of the present invention is short, and excellent UV resistance can be achieved, and it has durability.

[0005] The technical solution adopted by the present invention is:

[0006] The processing method of the anti-ultraviolet lyocell fabric comprises the following fabric finishing process: alkali treatment→mechanical polishing→fixation treatment; the alkali treatment process comprises the following steps: treatment temperature of 90-95°C, treatment time of 15-18 minutes, and working liquid composition of 60-75 g / L sodium carbonate (pH value adjusted within the range of 8.5-9), 3-4 g / L chelating agent, 3-5 g / L penetrant, and the balance of water.

[0007] The mechanical grinding process is as follows: front side: large cylinder 70-75 rpm, tension 3-3.5 Bar, rotation speed 85-90 m / min, vehicle speed 40-45 m / min, back side: large cylinder 60-65 rpm, tension 3 Bar, rotation speed 70-75 m / min, vehicle speed 50-60 m / min.

[0008] The fixing treatment process has a temperature of 70-75°C, a treatment time of 8-10 minutes, and a working liquid composition of: 10-18 g / L sodium carbonate (pH value adjusted within the range of 7.5-8), 50-70 g / L benzotriazole compound containing acryloyl group, 3-5 g / L penetrant, 3-5 g / L pH stabilizer, and the balance is water.

[0009] The fabric specification is R120+P120*R120+P120*200*150*57 / 58. In order to achieve a better strength level without losing the lightness of Lyocell, the warp and weft arrangement ratio of Lyocell and polyester is 3:1, and the organization is 1 / 1.

[0010] In order to achieve a better level of strength without losing the lightness of Lyocell, the warp and weft patterns of Lyocell and polyester are designed in a ratio of 3:1.

[0011] In order to achieve the best anti-ultraviolet effect, mild alkali treatment is carried out to open the skin and core layers of the Lyocell fiber, and mechanical grinding equipment is used to enhance the specific surface area of ​​the fabric. Then, the benzotriazole compound containing acryl is fully attached to the fibers on the fabric for fixation.

[0012] The chelating agent is chelating agent SQ-A.

[0013] The penetrant is penetrant WA-M.

[0014] In the mechanical polishing process, a Lafer sanding machine, model Ultrasoft-Y, is used for mechanical polishing.

[0015] The benzotriazole compound containing acryl is an anti-ultraviolet additive SYS-SUN.

[0016] The pH stabilizer is stabilizer HP-AC.

[0017] The invention solves the problem of poor anti-ultraviolet effect of a plain ultra-light lyocell fabric with warp and weft yarn counts of 120s, a warp yarn density of 200 yarns / inch, and a weft yarn density of 150 yarns / inch. The invention designs the structure specification, designs lyocell and polyester in a warp and weft direction in a ratio of 3:1, and then immerses the pre-treated fabric in a sodium carbonate solution with a pH value of 8.5-9 and a temperature of 90-95°C for 15 minutes, performs mechanical polishing after drying, and then immerses the fabric in a mixed solution of sodium carbonate with a pH value of 7.5-8 and a benzotriazole compound containing an acryl group with a concentration of 50-70g / L for 10 minutes at a treatment temperature of 70-75°C. The anti-ultraviolet effect of the treated fabric is greatly improved, and the UPF value can be increased from 15 of an untreated fabric to more than 50.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] Through tissue specification design, mild alkali treatment and fixation of benzotriazole compounds containing acryloyl groups on the fabric after mechanical polishing, the UPF value is greatly improved from 15 before treatment to more than 50. The process of the present invention is short, and can achieve excellent anti-ultraviolet performance and durability. The UPF value of the fabric can still reach more than 50 after 30 washes. DETAILED DESCRIPTION

[0020] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.

[0021] Raw materials used in embodiments and comparative examples:

[0022] Chelating agent SQ-A is a commercial product of Zibo Lurui Fine Chemical Co., Ltd.

[0023] Penetrant WA-M is a commercially available product of Zibo Lurui Fine Chemical Co., Ltd.

[0024] Anti-ultraviolet additive SYS-SUN is a commercial product of Zibo Lurui Fine Chemical Co., Ltd.

[0025] Stabilizer HP-AC is a commercially available product of Qingdao Furuiqi Textile New Materials Co., Ltd.

[0026] Test method:

[0027] Anti-ultraviolet testing method: tested according to GB / T 18830-2009;

[0028] Breaking strength test method: tested according to ASTM D5034-09 (R2013).

[0029] Example 1

[0030] Fabric specifications: R120+P120*R120+P120*200*150*57 / 58, structure: 1 / 1, the warp and weft arrangement of lyocell and polyester are in the ratio of 3:1.

[0031] The fabric finishing process is: alkali treatment → mechanical polishing → fixation treatment.

[0032] The specific steps are as follows:

[0033] (1) Alkali treatment process, the treatment temperature is 95 ° C, the treatment time is 15 min, and the working solution composition is: sodium carbonate 75 g / L, SQ-A 4 g / L, WA-M 5 g / L, and the balance is water;

[0034] (2) Mechanical grinding process, front side: large cylinder 75 rpm, tension 3.5 Bar, speed 90 m / min, vehicle speed 45 m / min, back side: large cylinder 65 rpm, tension 3 Bar, speed 75 m / min, vehicle speed 60 m / min;

[0035] (3) Fixing treatment process: the treatment temperature is 75°C, the treatment time is 8 min, and the working liquid composition is: sodium carbonate 18 g / L, SYS-SUN 70 g / L, WA-M 5 g / L, HP-AC 5 g / L, and the balance is water.

[0036] Example 2

[0037] Fabric specifications: R120+P120*R120+P120*200*150*57 / 58, structure: 1 / 1, the warp and weft arrangement of lyocell and polyester are in the ratio of 3:1.

[0038] The fabric finishing process is: alkali treatment → mechanical polishing → fixation treatment.

[0039] The specific steps are as follows:

[0040] (1) Alkali treatment process, the treatment temperature is 90 ° C, the treatment time is 18 min, and the working solution composition is: sodium carbonate 60 g / L, SQ-A 3 g / L, WA-M 3 g / L, and the balance is water;

[0041] (2) Mechanical grinding process, front side: large cylinder 70 rpm, tension 3 Bar, speed 85 m / min, speed 40 m / min, back side: large cylinder 60 rpm, tension 3 Bar, speed 70 m / min, speed 50 m / min;

[0042] (3) Fixing treatment process: the treatment temperature is 70°C, the treatment time is 10 min, and the working liquid composition is: sodium carbonate 10 g / L, SYS-SUN 50 g / L, WA-M 3 g / L, HP-AC 3 g / L, and the balance is water.

[0043] Comparative Example 1

[0044] The fabric used in this comparative example has the same spinning method, the same specifications, and the same organization as the fabric in Example 1: 1 / 1, but the warp and weft arrangement of lyocell and polyester are both in a ratio of 4:1.

[0045] The fabric finishing process is exactly the same as in Example 1.

[0046] Comparative Example 2

[0047] The fabric used in this comparative example has the same spinning method, the same specifications, and the same organization as the fabric in Example 1: 1 / 1, but the warp and weft patterns of lyocell and polyester are arranged in a ratio of 1:1.

[0048] The fabric finishing process is exactly the same as in Example 1.

[0049] Comparative Example 3

[0050] The fabric used in this comparative example is exactly the same as the fabric used in Example 1.

[0051] The fabric finishing process flow is different from that of Example 1 only in that the comparative example 3 does not perform the alkali treatment step, and the rest of the process flows are the same.

[0052] Comparative Example 4

[0053] The fabric used in this comparative example is exactly the same as the fabric in Example 1.

[0054] The fabric finishing process flow is different from that of Example 1 only in that the mechanical polishing step is not performed in Comparative Example 3, and the rest of the process flows are the same.

[0055] Comparative Example 5

[0056] The fabric used in this comparative example is exactly the same as the fabric used in Example 1.

[0057] The fabric finishing process flow is different from that of Example 1 only in that: Comparative Example 3 does not use sodium carbonate and HP-AC to control the pH value, and the pH value of this working solution is about 9.5. The rest of the process flows are the same.

[0058] The fabrics of Examples 1-2 and Comparative Examples 1-4 were subjected to performance tests, and the test results are shown in Table 1.

[0059] Table 1 Performance test results

[0060]

[0061] Although comparative example 1 also has extremely high UV resistance, its breaking strength is only 11.6LB, and there is a high risk of fabric breakage, holes, etc. during processing. As clothing, it is also very easy to have poor wear resistance and the fabric will crack during pulling. In summary, comparative example 1 is not suitable as a processing method for UV-resistant lyocell fabrics.

Claims

1. A method for processing an anti-ultraviolet lyocell fabric, characterized in that: The fabric finishing process is: alkali treatment → mechanical polishing → fixation treatment. The alkali treatment process: the treatment temperature is 90-95°C, the treatment time is 15-18min, and the working liquid composition is: sodium carbonate 60-75g / L, chelating agent 3-4 g / L, penetrant 3-5g / L, and the balance is water; In the mechanical grinding process, the front side: large cylinder 70-75 rpm, tension 3-3.5 Bar, rotation speed 85-90 m / min, vehicle speed 40-45 m / min, the back side: large cylinder 60-65 rpm, tension 3 Bar, rotation speed 70-75 m / min, vehicle speed 50-60 m / min; In the fixing treatment process, the temperature is 70-75°C, the treatment time is 8-10 minutes, and the working liquid composition is: 10-18 g / L sodium carbonate, 50-70 g / L benzotriazole compound containing acryloyl group, 3-5 g / L penetrant, 3-5 g / L pH stabilizer, and the balance is water, and the pH value is adjusted to be in the range of 7.5-8; The fabric specifications are R120+P120* R120+P120*200*150*57 / 58, the warp and weft pattern ratio of lyocell and polyester is 3:1, and the weft pattern ratio is 1 / 1. The pH stabilizer is stabilizer HP-AC.

2. The processing method of the anti-ultraviolet lyocell fabric according to claim 1, characterized in that: The chelating agent is chelating agent SQ-A.

3. The processing method of the anti-ultraviolet lyocell fabric according to claim 1, characterized in that: The penetrant is penetrant WA-M.

4. The processing method of the anti-ultraviolet lyocell fabric according to claim 1, characterized in that: In the mechanical polishing process, a Lafer sanding machine is used for mechanical polishing.

5. The processing method of the anti-ultraviolet lyocell fabric according to claim 1, characterized in that: The benzotriazole compound containing acryl is an anti-ultraviolet additive SYS-SUN.

Citation Information

Patent Citations

  • Production process of high-density high-elasticity health fabric

    CN106521786A

  • Recycling of man-made cellulosic fibers

    CN107208325A