A roadbed dry-wet cycle damage test device and damage calculation method

By designing a roadbed dry-wet cycle damage experimental device and corresponding evaluation methods, the problem of the inability to effectively evaluate the roadbed dry-wet cycle damage in the existing technology has been solved, achieving accurate quantification and evaluation of roadbed damage, and improving the efficiency and effectiveness of road construction. Material utilization.

CN115855650BActive Publication Date: 2024-10-11XIFU BRANCH OF SHIJIAZHUANG JIAOJIAN EXPRESSWAY CONSTR MANAGEMENT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211553035.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-10-11
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

The existing technology lacks an effective method to evaluate and quantify the damage of the roadbed under the action of dry and wet cycles, especially on roads that have been washed by water for a long time, resulting in the inability to accurately assess the damage of the roadbed.

Method used

A roadbed dry-wet cycle damage experimental device is designed, which includes a cylindrical fixed outer ring and an arc-shaped pressure plate, combined with a damper and a pressure spring, to simulate the confining pressure environment of the roadbed, and proposes a dry-wet cycle damage evaluation Method: Through the dry-wet cycle treatment and uniaxial compression test of earthwork specimens, the damage evaluation index Ki of the roadbed was calculated.

Benefits of technology

The device and method can accurately simulate the confining pressure environment of the subgrade, obtain the stress-strain curve, provide a quantitative evaluation of the subgrade damage, help evaluate the damage of the subgrade material, and determine whether the old subgrade can be reused, thereby improving construction efficiency and saving Material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115855650B_ABST
    Figure CN115855650B_ABST
Patent Text Reader

Abstract

The present invention provides a roadbed dry-wet cycle damage test device and a damage calculation method, wherein the damage test device includes a cylindrical fixed outer ring, a plurality of arc-shaped pressure plates are arranged inside the fixed outer ring, and the plurality of arc-shaped pressure plates surround a cylindrical movable pressure ring, the movable pressure ring is coaxially arranged with the fixed outer ring, and a plurality of dampers and a plurality of pressure springs are connected between the fixed outer ring and the arc-shaped pressure plate. The damage test device of the present invention can provide confining pressure for earthwork specimens made of experimental roadbed materials, so that the experimental conditions are closer to the real environment, thereby making the experimental results more accurate. In addition, the damage calculation method of the present invention is based on the roadbed linear / nonlinear theory, considering the linear-elastic-plastic properties of roadbed materials, and the calculation results are accurate. The dry-wet cycle damage calculation method provided by the present invention can accurately determine the dry-wet cycle damage of roadbed materials, and provide a basis for determining whether the old roadbed can be used again.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of roadbed evaluation, in particular to a roadbed dry-wet cycle damage experimental device and a damage calculation method. Background Art

[0002] Most roadbeds are built with earth. Under the action of vehicle loads, the roadbed not only bears compressive stress and horizontal force, but also bears the external environment, such as temperature, water, snow, wind, etc. In particular, some roadbeds are built along rivers. The roadbed is soaked in river water for a long time, and the internal materials of the roadbed will be damaged.

[0003] At present, there is no standard for the damage of roadbed due to dry-wet cycles. Under certain loads, many people think that as long as the deformation of the roadbed meets the standard, it is sufficient. However, the actual application is not ideal, and there is no evaluation index for flooded roadbed. Many roads are used as flood embankments (one side of the road is a river), and these places are eroded by water for a long time. There is no definite method to conduct a specific evaluation of the roadbed, and the dry-wet damage of the roadbed cannot be quantified. Summary of the invention

[0004] One of the purposes of the present invention is to provide a roadbed dry-wet cycle damage test device for roadbed dry-wet cycle damage test.

[0005] The second purpose of the present invention is to provide a method for calculating the dry-wet cycle damage of the roadbed, so as to quantify the roadbed damage and thus realize the specific evaluation of the roadbed.

[0006] One of the purposes of the present invention is achieved as follows: a roadbed dry-wet cycle damage test device includes a cylindrical fixed outer ring, a plurality of arc-shaped pressure plates are arranged inside the fixed outer ring, and the plurality of arc-shaped pressure plates form a cylindrical movable pressure ring, the movable pressure ring is coaxially arranged with the fixed outer ring, and a plurality of dampers and a plurality of pressure springs are connected between the fixed outer ring and the arc-shaped pressure plate.

[0007] The plurality of dampers and the plurality of pressure springs are alternately arranged in rows along the circumference of the fixed outer ring, and the number of dampers in each row is equal, and the number of pressure springs in each row is equal.

[0008] Furthermore, a row of pressure springs and dampers are respectively provided between the inner wall of the fixed outer ring and each arc-shaped pressure plate.

[0009] Furthermore, in step c, the experimental device is provided with eight arc-shaped pressure plates.

[0010] The second object of the present invention is achieved as follows: A method for evaluating roadbed dry-wet cycle damage comprises the following steps:

[0011] a. The materials for roadbed to be evaluated are made into several earthwork specimens according to the dry and wet damage test specifications and left to dry naturally;

[0012] b. Divide the earthwork specimens into several groups according to the number of dry-wet cycles, and perform dry-wet cycle treatment on the grouped earthwork specimens. The number of dry-wet cycles for each group of earthwork specimens is equal; each dry-wet cycle is to soak the earthwork specimens and then let them stand for 48 hours;

[0013] c. Prepare the roadbed dry-wet cycle damage test device as claimed in claim 1; the inner diameter of the movable pressure ring of the test device is smaller than the diameter of the earthwork specimen;

[0014] d. Place the earthwork specimens in the movable pressure ring of the experimental device in the previous step in sequence. The pressure value generated by the combined action of the pressure spring and damping of the experimental device is equal to the actual confining pressure of the roadbed. After the earthwork specimens are placed, a uniaxial compression test is performed to obtain the stress-strain curve of each group of earthwork specimens.

[0015] e. Mark a straight line segment of the approximate straight line in each set of stress-strain curves obtained, and mark the coordinate values ​​of the starting point and the end point of the straight line segment, and calculate the elastic modulus of the straight line segment, which is recorded as E i , where i is the number of dry-wet cycles;

[0016] f. Calculate the evaluation index K of roadbed dry-wet cycle damage i :

[0017] K i =(E1-E i ) / E1

[0018] Among them, E1 is the elastic modulus of the earthwork specimen group subjected to one dry-wet cycle treatment;

[0019] g. The obtained evaluation index K i The corresponding relationship between the dry-wet cycle damage evaluation index and the evaluation result is compared to obtain the evaluation result of the roadbed material to be evaluated.

[0020] Preferably, the number of earthwork specimens in each group is equal.

[0021] In step c, the plurality of dampers and the plurality of pressure springs of the experimental device are alternately arranged in rows along the circumference of the fixed outer ring, and the number of dampers in each row is equal, and the number of pressure springs in each row is equal.

[0022] A row of pressure springs and dampers are respectively provided between the inner wall of the fixed outer ring of the experimental device and each arc-shaped pressure plate.

[0023] Preferably, eight arc-shaped pressure plates are provided.

[0024] The present invention provides a roadbed dry-wet cycle damage test device, which can truly simulate the confining pressure environment of the roadbed and ensure the accuracy of the stress-strain curve obtained by the uniaxial compression test. In addition, the present invention provides a roadbed dry-wet cycle damage evaluation method, which is based on the roadbed linear / nonlinear theory and takes into account the linear-elastic-plastic deformation of the roadbed material, so that the measured stress-strain curve of the roadbed material is more accurate. The roadbed dry-wet cycle damage evaluation method proposed in the present invention can accurately evaluate the roadbed, and the method can also be used to evaluate the old roadbed to determine whether the old roadbed can be used again, thereby saving construction materials and improving road construction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a structural schematic diagram of the present invention.

[0026] Figure 2 It is the stress-strain curve under different numbers of drying and wetting cycles.

[0027] In the figure: 1. pressure spring; 2. damper; 3. arc pressure plate; 4. fixed outer ring. DETAILED DESCRIPTION

[0028] Example 1 A roadbed dry-wet cycle damage test device

[0029] like Figure 1 As shown, the present invention provides a roadbed dry-wet cycle damage test device, which includes a cylindrical fixed outer ring 4, a plurality of arc-shaped pressure plates 3 are arranged inside the fixed outer ring 4, and the plurality of arc-shaped pressure plates 3 form a cylindrical movable pressure ring inside the fixed outer ring 4, and the movable pressure ring is coaxially arranged with the fixed outer ring. A damper 2 and a pressure spring 1 are connected between the fixed outer ring 4 and the arc-shaped pressure plate 3, and a plurality of dampers 2 and pressure springs 1 are provided. There are 8 arc-shaped pressure plates 3 in this embodiment, and gaps are left between them.

[0030] In addition, the dampers 2 and the pressure springs 1 in this embodiment are arranged alternately in rows along the circumference of the fixed outer ring 4, and the number of dampers 2 in each row is equal, and the number of pressure springs 1 in each row is equal. In this embodiment, the pressure springs 1 and dampers 2 connected between the fixed outer ring 4 and each arc-shaped pressure plate are each provided with one row. In addition, the models of the pressure springs 1 and dampers 2 in the present invention can be determined according to the size of the confining pressure to be generated, so as to expand the application range of the device.

[0031] Example 2 A method for evaluating roadbed dry-wet cycle damage

[0032] The present invention provides a method for evaluating roadbed dry-wet cycle damage, the method comprising the following steps:

[0033] S1. First, the roadbed material to be evaluated is made into several earthwork specimens with a size of Φ61.8mm×125mm according to the dry-wet test specifications, and then placed to dry naturally.

[0034] S2. Divide the naturally dried earthwork specimens into several groups according to the number of dry-wet cycles, and perform dry-wet cycle treatment on the grouped earthwork specimens, and the number of dry-wet cycles of each group of earthwork specimens is equal. In this embodiment, 33 earthwork specimens are made, and the 33 earthwork specimens are divided into 11 groups, and 3 earthwork specimens are set in each group. The 11 groups of earthwork specimens are subjected to 1, 2, 3, 4, 5, 6, 9, 12, 15, 18, and 21 dry-wet cycles respectively. Each dry-wet cycle treatment is to soak the earthwork specimen and then let it stand for 48 hours. Generally, the humidification part of the earthwork specimen is located at the top or bottom of the specimen to match the actual situation.

[0035] S3. Prepare the roadbed dry-wet cycle damage test device described in Example 1. The specific structure of the device is not introduced in detail here. The inner diameter of the movable inner ring of the test device should be smaller than the diameter of the earthwork specimen to ensure that the earthwork specimen is initially subjected to confining pressure, so as to be closer to the actual situation.

[0036] S4, the earthwork specimens are sequentially placed in the movable pressure ring of the experimental device prepared in the previous step, and the pressure value generated by the combined action of the pressure spring 1 and the damper 2 of the experimental device is equal to the actual confining pressure of the roadbed. After the earthwork specimens are placed, a uniaxial compression test is performed to obtain the stress-strain curve of the earthwork specimens. In this step, during uniaxial compression, as the earthwork specimens deform, under the action of the pressure spring 1 and the damper 2, the compressed earthwork specimens receive a confining pressure that is close to the actual situation, so that the obtained stress-strain curve is more accurate.

[0037] S5. Obtain an average stress-strain curve for each set of earthwork specimens. Mark a straight line segment that approximates a straight line in the obtained stress-strain curve, and mark the starting point and end point of the straight line segment. The marked stress-strain curve is as follows: Figure 2 As shown, record the coordinates of the starting point (ε iA , σ iA ) and the end point coordinates (ε iB , σ iB ), calculate the elastic modulus of the marked straight line segment, denoted as Ei:

[0038]

[0039] Where i is the number of dry-wet cycles.

[0040] S6. Calculation of the roadbed dry-wet cycle damage evaluation index K i :

[0041] K i =(E1-Ei ) / E1

[0042] Among them, E1 is the elastic modulus of the earthwork specimen group subjected to one dry-wet cycle treatment.

[0043] The K obtained in this embodiment i The specific values ​​are shown in Table 1.

[0044] Table 1 Damage index K of different dry-wet cycles i value

[0045]

[0046] S7, the obtained evaluation index K i The corresponding relationship between the dry-wet cycle damage evaluation index and the evaluation result is compared to obtain the evaluation result of the roadbed material to be evaluated. The corresponding relationship between the dry-wet cycle damage evaluation index and the evaluation result in this embodiment is shown in Table 2. By comparison, the following conclusion can be drawn about the roadbed material in this embodiment: the roadbed material is excellent if it has less than 6 dry-wet cycles, and it is qualified if it has less than 21 dry-wet cycles.

[0047] Table 2 Correspondence between dry-wet cycle evaluation indicators and evaluation results

[0048]

[0049] The relationship between the dry-wet cycle evaluation index K and the evaluation results in the above table is obtained by comparing the evaluation index obtained after repeated dry-wet cycle treatments with the actual damage of the roadbed material after dry-wet cycles.

[0050] In order to verify the accuracy of this method, a verification test was conducted. The verification test used the same roadbed material as in this facility example and conducted the same dry-wet cycle experiment as in this example under the same conditions. The dry-wet cycle evaluation index K i The values ​​are shown in Table 3.

[0051] It can be seen from Table 3 that the dry-wet cycle damage evaluation index K obtained by the control group i Damage evaluation index K for the same number of dry-wet cycles as in Table 1 i The values ​​are almost equal, so the evaluation result obtained by the evaluation method of the present invention is stable and reliable.

[0052] Table 3 Damage evaluation index D of different dry-wet cycle times in the experimental group i value

[0053]

Claims

1. A method for evaluating roadbed dry-wet cycle damage, characterized in that: The following steps are involved: a. The materials for roadbed to be evaluated are made into several earthwork specimens according to the dry and wet damage test specifications and left to dry naturally; b. Divide the earthwork specimens into several groups according to the number of dry-wet cycles, and perform dry-wet cycle treatment on the grouped earthwork specimens. The number of dry-wet cycles for each group of earthwork specimens is equal; each dry-wet cycle is to soak the earthwork specimens and then let them stand for 48 hours; c. Prepare a roadbed dry-wet cycle damage test device, the test device comprises a cylindrical fixed outer ring, a plurality of arc-shaped pressure plates are arranged inside the fixed outer ring, the plurality of arc-shaped pressure plates surround a cylindrical movable pressure ring, the movable pressure ring is coaxially arranged with the fixed outer ring, a plurality of dampers and a plurality of pressure springs are connected between the fixed outer ring and the arc-shaped pressure plates, the plurality of dampers and the plurality of pressure springs are alternately arranged in rows along the circumference of the fixed outer ring, the number of dampers in each row is equal, the number of pressure springs in each row is equal, and the pressure springs and dampers connected between the inner wall of the fixed outer ring and each arc-shaped pressure plate are respectively arranged in one row; the inner diameter of the movable pressure ring of the test device is smaller than the diameter of the earthwork specimen; d. Place the earthwork specimens in the movable pressure ring of the experimental device in the previous step in sequence. The pressure value generated by the combined action of the pressure spring and the damper of the experimental device is equal to the actual confining pressure of the roadbed. After the earthwork specimens are placed, a uniaxial compression test is performed to obtain the stress-strain curve of each group of earthwork specimens. e. In each set of stress-strain curves obtained, mark a straight line segment that approximates a straight line, and mark the coordinate values ​​of the starting point and the end point of the straight line segment, and calculate the elastic modulus of the straight line segment, which is recorded as , where i is the number of dry-wet cycles; f. Calculate the evaluation index of roadbed dry-wet cycle damage : ; in, is the elastic modulus of the earthwork specimen group subjected to one dry-wet cycle treatment; g. The evaluation indicators obtained The corresponding relationship between the dry-wet cycle damage evaluation index and the evaluation result is compared to obtain the evaluation result of the roadbed material to be evaluated.

2. The method for evaluating roadbed dry-wet cycle damage according to claim 1, characterized in that: The number of earthwork specimens in each group is equal.

3. The method for evaluating roadbed dry-wet cycle damage according to claim 1, characterized in that: In step c, the experimental device is provided with eight arc-shaped pressure plates.

Citation Information

Patent Citations

  • Triaxial test device and test method for simulating wet and dry circulation of rock in fluctuation zone of reservoir

    CN102435480A

  • Nondestructive prediction combination method for evaluating rock uniaxial compressive strength under freeze-thaw cycle

    CN110987748A

  • Method for accurately measuring compressive strength of concrete material in variable confining pressure state

    CN111912709A

  • Dry-wet cycle triaxial testing machine and use method thereof

    CN112834320A

  • Rock-soil body volume change testing and measuring device and method under low triaxial stress and water seepage conditions

    CN115184142A