A rare earth rotating target material and its preparation method and application

By forming a composite structure of the back tube and powdered raw materials, performing cold isostatic pressing or hot isostatic pressing, and controlling the temperature difference, efficient welding and integrated forming of the rare earth rotating target material is achieved, which solves the problem of target tube preparation and welding in the existing technology. It solves the problems of low efficiency and open welding, improves the welding rate and preparation efficiency, and meets the application needs in the fields of magnetic material coating and electronic information.

CN115874155BActive Publication Date: 2024-10-11GRIREM ADVANCED MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111151674.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-29
Publication Date
2024-10-11
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Existing preparation methods for rare earth metal or alloy rotating targets fail to achieve target tube preparation and welding at the same time, resulting in low welding efficiency, high consumption of solder such as indium, low welding rate, and easy welding during use.

Method used

By forming the back tube and the powdered raw material into a composite structure, performing cold isostatic pressing or hot isostatic pressing, and controlling the temperature difference during the material stratification and cooling processes, the target tube and the back tube are welded and integrated into one. A preparation method.

Benefits of technology

It improves the welding rate and preparation efficiency of the rare earth rotating target, saves solder consumption, and ensures that the target will not be welded during use, meeting the application needs of magnetic material coating grain boundary diffusion, storage and electronic information fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115874155B_ABST
    Figure CN115874155B_ABST
Patent Text Reader

Abstract

A rare earth rotating target material and its preparation method and application, the method comprising: placing a back tube and powdered raw materials into a mold to form a composite structure with a back tube in the center and raw material layers around, wherein the raw materials include rare earth metal single substance and / or rare earth alloy, the raw material layers include a first raw material layer and a second raw material layer, the first raw material layer is located between the back tube and the second raw material layer, and the raw material particle size in the first raw material layer is smaller than the raw material particle size in the second raw material layer; cold / hot isostatic pressing is performed on the composite structure, and the temperature difference between the back tube and the raw material layer is controlled during the sintering cooling process to obtain a rare earth rotating target material. The method combines the two steps of target tube preparation and welding into one, and simultaneously realizes the welding of the target tube and the back tube during the preparation process of the rare earth rotating target tube, which not only shortens the preparation process of rare earth metal and alloy rotating targets, improves the preparation efficiency, but also saves solders such as indium, and solves the problems of low welding rate and target material open welding in the later stage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of rotary target materials, and in particular to a rare earth metal or rare earth alloy rotary target material and an integrated molding preparation method and application thereof. Background Art

[0002] Magnetron sputtering technology uses the collision between incident particles and target materials for coating, where the target materials can be divided into planar targets, tubular targets or rotating targets, etc. At present, the utilization rate of rare earth metal and rare earth alloy planar targets is generally 30-50wt%, while the utilization rate of tubular targets or rotating targets is as high as 80wt% or more, which is more suitable for magnetic material coating grain boundary diffusion, storage and electronic information and other fields, and the future market demand is huge.

[0003] The rotating target must be combined with the target tube and the back tube before it can be used for magnetron sputtering. Currently, welding is usually used to combine the two. The rotating target material obtained by welding needs to not open during use and have good thermal conductivity so that the heat generated by the magnetron sputtering process can be taken away in time. In order to meet the above-mentioned use requirements, the welding rate of the rotating target material must be above 95%. In order to meet the above-mentioned use requirements as much as possible, the existing preparation method of rare earth metal or alloy rotating targets includes: the first step is to prepare the blank by melting or powder metallurgy, and process it into a target tube, and the second step is to connect the target tube and the back tube together by solder to obtain the target material. However, the existing preparation method fails to achieve the simultaneous preparation of the target tube and welding. Not only does welding require more solders such as indium, but the preparation efficiency of the rotating target is low, the process is long, and the welding rate is still not high enough. Summary of the invention

[0004] (I) Purpose of the invention

[0005] The purpose of the present invention is to provide a rare earth rotary target material and a preparation method and application thereof. The method combines the two steps of target tube preparation and welding into one, and by controlling the material stratification, the particle size difference of each layer and the temperature difference between the back tube and the raw material layer during the cooling process, not only the problems of low welding rate of the rotary target material and open welding during use are solved, but also the welding of the target tube and the back tube is realized during the preparation of the rare earth rotary target tube, thereby shortening the preparation process of rare earth metal and alloy rotary targets, improving the preparation efficiency, and saving solders such as indium.

[0006] (II) Technical solution

[0007] In order to solve the above problems, the first aspect of the present application provides a method for preparing a rare earth rotating target, comprising:

[0008] Putting a backing tube and a powdered raw material into a mold to form a composite structure with the backing tube in the center and raw material layers around it, wherein the raw material includes a rare earth metal element and / or a rare earth alloy, and the raw material layers include a first raw material layer and a second raw material layer, the first raw material layer is located between the backing tube and the second raw material layer, and the raw material particle size in the first raw material layer is smaller than the raw material particle size in the second raw material layer;

[0009] The composite structure is subjected to cold isostatic pressing or hot isostatic pressing to obtain a rare earth rotating target material, wherein the cold isostatic pressing process includes cold isostatic pressing to obtain a blank and sintering the blank, and during the cooling process of the cold isostatic pressing process and the hot isostatic pressing, a certain temperature difference is controlled between the back tube and the raw material layer to obtain a rare earth rotating target material. The method combines the two steps of target tube preparation and welding into one, realizes the efficient preparation of the rare earth rotating target tube and the back tube welded into one body, not only shortens the preparation process of rare earth metal and alloy rotating targets, but also saves solders such as indium, and solves the problems of low welding rate of rotating targets and open welding during use.

[0010] Specifically, the thickness of the first raw material layer is 0.1-1 mm, the particle size of the raw material in the first raw material layer is 1-100 μm, and the particle size of the raw material in the second raw material layer is 10-150 μm;

[0011] The particle size of the raw material in the second raw material layer is 2 to 3 times the particle size of the raw material in the first raw material layer.

[0012] In a specific embodiment, the specific conditions of cold isostatic pressing include:

[0013] The pressure is 50-500MPa, and the holding time is 80-200min.

[0014] In an optional embodiment, the specific conditions for sintering the blank include:

[0015] Pressureless sintering in vacuum or inert atmosphere;

[0016] Sintering temperature T1 satisfies:

[0017] When T 原料 ≤T 背管 When T1 = 0.5 ~ 0.95T 原料 ;

[0018] When T 原料 >T 背管 When T1 = 0.5 ~ 0.95T 原料 , and T1<0.8T 背管 ;

[0019] The sintering time is 30 to 250 minutes;

[0020] Among them, T 原料 is the melting point of the raw material, T 背管 is the melting point of the back tube.

[0021] Furthermore, during the cooling process after sintering, the temperature difference between the back tube and the raw material layer is controlled to be 50-300°C, that is, the temperature difference T between the back tube and the raw material layer is controlled to be X -T d =50~300℃, where T x T is the temperature of the one with smaller expansion coefficient between the back tube and the raw material layer, d It is the temperature of the one with the larger expansion coefficient between the back tube and the raw material layer.

[0022] In another optional embodiment, the specific conditions for sintering the blank include:

[0023] Perform hot isostatic pressing sintering;

[0024] The sintering pressure is 5-50MPa;

[0025] Sintering temperature T1 satisfies:

[0026] When T 原料 ≤T 背管 When T1 = 0.5 ~ 0.9T 原料 ;

[0027] When T 原料 >T 背管 When T1 = 0.5 ~ 0.9T 原料 , and T1<0.8T 背管 ;

[0028] The sintering time is 30 to 240 minutes;

[0029] Among them, T 原料 is the melting point of the raw material, T 背管 is the melting point of the back tube.

[0030] Furthermore, during the cooling process after sintering, the temperature difference between the back tube and the raw material layer is controlled to be 50-300°C, that is, the temperature difference T between the back tube and the raw material layer is controlled to be X -T d =50~300℃, where T x T is the temperature of the one with smaller expansion coefficient between the back tube and the raw material layer, d It is the temperature of the one with the larger expansion coefficient between the back tube and the raw material layer.

[0031] In another specific embodiment, the composite structure is subjected to hot isostatic pressing, which specifically includes:

[0032] Performing hot isostatic pressing sintering on the composite structure;

[0033] The sintering pressure is 10~60MPa;

[0034] Sintering temperature T1 satisfies:

[0035] When T 原料 ≤T 背管 When T1 = 0.5 ~ 0.9T 原料 ;

[0036] When T 原料 >T 背管 When T1 = 0.5 ~ 0.9T 原料 , and T1<0.8T 背管 ;

[0037] The sintering time is 30 to 270 minutes;

[0038] Among them, T 原料 is the melting point of the raw material, T 背管 is the melting point of the back tube.

[0039] Furthermore, during the cooling process after the hot isostatic pressing sintering is completed, the temperature difference T between the back tube and the raw material layer is controlled. X -T d =50~300℃, where T x T is the temperature of the one with smaller expansion coefficient between the back tube and the raw material layer, d It is the temperature of the one with the larger expansion coefficient between the back tube and the raw material layer.

[0040] In a second aspect of the present application, a rare earth rotating target prepared by any of the preparation methods described above is provided.

[0041] The third aspect of the present application provides the application of the rare earth rotating target prepared by any of the preparation methods described above in the fields of magnetic material coating grain boundary diffusion, storage and electronic information.

[0042] (III) Beneficial effects

[0043] The above technical solution of the present invention has the following beneficial technical effects:

[0044] The preparation method of the rare earth rotary target material provided by the present invention comprises the following steps: placing a back tube and a powdered raw material into a mold together to form a composite structure with the back tube at the center and raw material layers around it; cold isostatic pressing, sintering or directly isostatic pressing the composite structure to achieve target tube molding and target tube / back tube binding at the same time; controlling the particle size of the inner layer raw material to be smaller than the particle size of the outer layer raw material to obtain better welding quality, thereby ensuring that a higher density and welding rate are obtained during the target tube molding process; controlling the temperature difference between the raw material layer and the back tube during the cooling process of sintering to effectively solve the problem of target material open welding in the later stage due to the large difference in expansion coefficient between the back tube and the rare earth target tube, thereby ensuring that the rotary target does not open welding during use; the method simultaneously realizes target material molding and welding, thereby obtaining a rotary target material with a density and welding rate that meet use requirements.

[0045] This method combines the two steps of target tube preparation and welding into one, and realizes the welding of the target tube and the back tube during the preparation of the rare earth rotating target tube. It not only shortens the preparation process of rare earth metal and alloy rotating target materials and improves the preparation efficiency, but also saves solders such as indium, and solves the problems of low welding rate of rotating targets and open welding during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is a schematic diagram of a composite structure provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0047] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0048] The present invention provides a method for preparing a rare earth rotating target material, comprising:

[0049] like Figure 1 As shown, a back tube and a powdered raw material are placed in a mold to form a composite structure with a back tube A in the center and raw material layers around it, wherein the raw material includes a rare earth metal element and / or a rare earth alloy, and the raw material layers include a first raw material layer B and a second raw material layer C, wherein the first raw material layer B is located between the back tube A and the second raw material layer C, and the raw material particle size in the first raw material layer B is smaller than the raw material particle size in the second raw material layer C;

[0050] The composite structure is subjected to cold isostatic pressing or hot isostatic pressing to obtain a rare earth rotating target material, wherein the cold isostatic pressing process includes cold isostatic pressing to obtain a blank and sintering the blank, and during the cooling process of the cold isostatic pressing process and the hot isostatic pressing, a certain temperature difference between the back tube and the raw material layer is controlled to obtain a rare earth rotating target material.

[0051] Specifically, the present invention can form a temperature difference between the back tube and the raw material layer during the cooling process by controlling the cooling rate of the sintering furnace, introducing a cooling medium into the center of the back tube and / or adding an auxiliary heating device, and the specific method is not limited in the present invention.

[0052] Specifically, the back tube in the present invention can be selected from stainless steel tubes, copper tubes, alloy tubes, titanium tubes, etc. as needed, preferably stainless steel tubes and titanium tubes; the rare earth metal element is selected from at least one of Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu; the rare earth alloy is an alloy of the above rare earth metal elements or multiple rare earth metals with metals such as Al, Cu, and Fe.

[0053] Specifically, the raw material can be degassed and the backing tube can be cleaned before preparation; the mold of the present invention can be a conventional isostatic soft mold. In an optional embodiment, in order to facilitate the formation of two layers of raw material, the mold also includes a thin-walled cylindrical auxiliary mold with an inner diameter slightly larger than the outer diameter of the backing tube. When the backing tube and the powdered raw material are placed in the mold, the backing tube is first placed in the center of the mold, and then the auxiliary mold is coaxially placed with the backing tube. The first raw material layer is filled in the cavity between the auxiliary mold and the backing tube, and the second raw material layer is filled in the interlayer between the auxiliary mold and the mold. Then, the auxiliary mold is removed, and the second raw material layer continues to be filled with its raw material until the second raw material layer is compacted.

[0054] The preparation method of the rare earth rotary target material provided by the present invention comprises the following steps: placing a back tube and a powdered raw material into a mold together to form a composite structure with the back tube in the center and raw material layers around it; cold isostatic pressing, sintering or directly hot isostatic pressing the composite structure to achieve target tube molding and target tube / back tube binding at the same time; controlling the particle size of the inner layer raw material to be smaller than the particle size of the outer layer raw material to obtain better welding quality, thereby ensuring that a higher density and welding rate are obtained during the target tube molding process; controlling the temperature difference between the target tube and the raw material layer during the cooling process to effectively solve the problem of open welding of the target material in the later stage due to the large difference in expansion coefficient between the back tube and the rare earth target tube, thereby ensuring that the rotary target does not open weld during use; the method simultaneously realizes target material molding and welding, thereby obtaining a rotary target material with a density and a welding rate that meet use requirements.

[0055] This method combines the two steps of target tube preparation and welding into one, achieving efficient preparation of the rare earth rotating target tube and the back tube by welding them into one piece. It not only shortens the preparation process of rare earth metal and alloy rotating targets, but also saves solders such as indium, and solves the problems of low welding rate of rotating targets and open welding during use.

[0056] Specifically, the thickness of the first raw material layer is 0.1-1 mm, the particle size of the raw material in the first raw material layer is 1-100 μm, and the particle size of the raw material in the second raw material layer is 10-150 μm;

[0057] Specifically, in the present invention, the raw material particle size refers to the average particle size D50.

[0058] By controlling the particle size and thickness of the two layers of powder within the above range, the quality of the welding layer can be better controlled, which can not only ensure that the fine powder forms a diffusion layer with the backing tube, but also avoid the formation of brittle intermetallic compounds caused by the strong alloying of the first layer of powder and the backing tube, thereby further ensuring the welding rate of the target material.

[0059] Preferably, the particle size of the raw material in the second raw material layer is 2 to 3 times that of the raw material in the first raw material layer, so as to ensure that the density of the target material reaches more than 96% and the welding rate reaches more than 96%.

[0060] In a specific embodiment, the specific conditions of isostatic pressing include:

[0061] The pressure is 50-500MPa, and the holding time is 80-200min.

[0062] In an optional embodiment, the specific conditions for sintering the blank include:

[0063] Pressureless sintering in vacuum or inert atmosphere;

[0064] Sintering temperature T1 satisfies:

[0065] When T 原料 ≤T 背管 When T1 = 0.5 ~ 0.95T 原料 ;

[0066] When T 原料 >T 背管 When T1 = 0.5 ~ 0.95T 原料 , and T1<0.8T 背管 ;

[0067] The sintering time is 30 to 250 minutes;

[0068] Among them, T 原料 is the melting point of the raw material, T 背管 is the melting point of the back tube.

[0069] Furthermore, during the cooling process after sintering, the temperature difference between the back tube and the raw material layer is controlled to be 50-300° C.

[0070] In another optional embodiment, the specific conditions for sintering the blank include:

[0071] Perform hot isostatic pressing sintering;

[0072] The sintering pressure is 5-50MPa;

[0073] Sintering temperature T1 satisfies:

[0074] When T 原料 ≤T 背管 When T1 = 0.5 ~ 0.9T 原料 ;

[0075] When T 原料 >T 背管 When T1 = 0.5 ~ 0.9T 原料 , and T1<0.8T 背管 ;

[0076] The sintering time is 30 to 240 minutes;

[0077] Among them, T 原料 is the melting point of the raw material, T 背管 is the melting point of the back tube.

[0078] Furthermore, during the cooling process after sintering, the temperature difference between the back tube and the raw material layer is controlled to be 50-300° C.

[0079] Compared with cold isostatic pressing + sintering, cold isostatic pressing + hot isostatic pressing and sintering is beneficial to further improve the density, welding strength and welding rate, and is beneficial to reducing the sintering temperature.

[0080] In another specific embodiment, the hot isostatic pressing of the composite structure specifically includes:

[0081] Performing hot isostatic pressing sintering on the composite structure;

[0082] The sintering pressure is 10~60MPa;

[0083] Sintering temperature T1 satisfies:

[0084] When T 原料 ≤T 背管 When T1 = 0.5 ~ 0.9T 原料 ;

[0085] When T 原料 >T 背管 When T1 = 0.5 ~ 0.9T 原料 , and T1<0.8T 背管 ;

[0086] The sintering time is 30 to 270 minutes;

[0087] Among them, T 原料 is the melting point of the raw material, T 背管 is the melting point of the back tube.

[0088] Furthermore, during the cooling process after sintering, the temperature difference between the back tube and the raw material layer is controlled to be 50-300° C.

[0089] Compared with cold isostatic pressing + sintering, direct hot isostatic pressing and sintering can shorten the preparation process, save time and reduce energy consumption. At the same time, it can produce rotating targets with the same quality as cold isostatic pressing + sintering.

[0090] The following are specific embodiments of the present invention:

[0091] The raw materials used in each embodiment are all commercially available products.

[0092] Example 1

[0093] (1) Degassing Tb powder with a particle size of 30 μm and Tb powder with a particle size of 80 μm for standby use;

[0094] (2) The 304 stainless steel backing tube with an outer diameter of 90 mm is cleaned and dried for later use;

[0095] (3) placing the raw material powder processed in step (1) and the backing tube processed in step (2) into a mold under vacuum and sealing them to form a composite structure with the backing tube in the center and the raw material layer around it, wherein the inner layer of the raw material layer is a powder with a particle size of 30 μm, the outer layer is a powder with a particle size of 80 μm, the inner layer is 0.5 mm thick, and the outer layer is 9.5 mm thick;

[0096] (4) After completing step (3), the raw material and the back tube composite structure are subjected to cold isostatic pressing to obtain a blank, with a pressure of 250 MPa and a holding time of 120 min;

[0097] (5) The blank obtained in step (4) is subjected to vacuum sintering to obtain a rotating target at a temperature of 0.8T. m (T m =1356°C, melting point of raw materials), holding time 150min, during cooling process, the cooling rate in the sintering furnace is controlled to be 5°C / min (cooling rate of raw material layer), and cooling water is introduced into the back tube. The cooling rate of the back tube is controlled by dynamically adjusting the cooling water flow rate through the automatic temperature control device. The back tube is controlled to be 100°C lower than the temperature of the raw material layer (target tube), which is recorded as target material A1.

[0098] Comparative Examples 1 to 5

[0099] The preparation method is basically the same as that in Example 1, and the differences are shown in Table 1. The obtained rotary targets are sequentially recorded as target A1' to target A5'.

[0100] Table 1 Process parameters of Example 1 and Comparative Examples 1 to 5

[0101]

[0102]

[0103] Example 2

[0104] (1) Degassing a DyFe alloy powder (Dy mass ratio 80%) with a particle size of 30 μm and a DyFe alloy powder with a particle size of 80 μm for standby use;

[0105] (2) The 304 stainless steel backing tube with an outer diameter of 90 mm is cleaned and dried for later use;

[0106] (3) placing the raw material powder processed in step (1) and the backing tube processed in step (2) into a mold under vacuum and sealing them to form a composite structure with the backing tube in the center and the raw material layer around it, wherein the inner layer of the raw material layer is a powder with a particle size of 30 μm, the outer layer is a powder with a particle size of 80 μm, the inner layer is 0.5 mm thick, and the outer layer is 9.5 mm thick;

[0107] (4) After completing step (3), the raw material and the back tube composite structure are subjected to cold isostatic pressing to obtain a blank, the pressure is 210 MPa, and the holding time is 120 min;

[0108] (5) The blank obtained in step (4) is subjected to vacuum sintering to obtain a rotating target at a temperature of 0.8T. m (T m =890°C), the holding time is 150min, and the cooling rate in the sintering furnace is controlled to be 5°C / min (raw material layer cooling rate) during the cooling process, and cooling water is introduced into the back tube. The cooling water flow rate is dynamically adjusted by the automatic temperature control device to control the back tube cooling rate. The back tube is controlled to be 200°C lower than the raw material layer temperature, which is recorded as target B1.

[0109] Comparative Examples 6 to 10

[0110] The preparation method is basically the same as that in Example 2, and the differences are shown in Table 2. The obtained rotary targets are sequentially recorded as targets B1' to B5'.

[0111] Table 2 Process parameters of Example 2 and Comparative Examples 6 to 10

[0112]

[0113] Example 3

[0114] (1) Degassing Tb powder with a particle size of 30 μm and Tb powder with a particle size of 80 μm for standby use;

[0115] (2) The 304 stainless steel backing tube with an outer diameter of 90 mm is cleaned and dried for later use;

[0116] (3) placing the raw material powder processed in step (1) and the backing tube processed in step (2) into a mold under vacuum and sealing them to form a composite structure with the backing tube in the center and the raw material layer around it, wherein the inner layer of the raw material layer is a powder with a particle size of 30 μm, the outer layer is a powder with a particle size of 80 μm, the inner layer is 0.5 mm thick, and the outer layer is 9.5 mm thick;

[0117] (4) After completing step (3), the raw material and the back tube composite structure are subjected to cold isostatic pressing to obtain a blank, with a pressure of 250 MPa and a holding time of 120 min;

[0118] (5) The blank obtained in step (4) is subjected to hot isostatic pressing to obtain a rotating target at a temperature of 0.8T. m (T m =1356°C), pressure 30MPa, heat and pressure holding time 150min, during the cooling process, the cooling rate in the sintering furnace is controlled to be 5°C / min (raw material layer cooling rate), and cooling water is introduced into the back tube. The cooling water flow rate is dynamically adjusted by the automatic temperature control device to control the back tube cooling rate. The back tube is controlled to be 100°C lower than the raw material temperature, which is recorded as target A2.

[0119] Comparative Examples 11 to 15

[0120] The preparation method is basically the same as that in Example 3, and the differences are shown in Table 3. The obtained rotary targets are sequentially recorded as target A11' to target A15'.

[0121] Table 3 Process parameters of Example 3 and Comparative Examples 11 to 15

[0122]

[0123]

[0124] Example 4

[0125] (1) Degassing a DyFe alloy powder (Dy mass ratio 80%) with a particle size of 30 μm and a DyFe alloy powder with a particle size of 80 μm for standby use;

[0126] (2) The 304 stainless steel backing tube with an outer diameter of 90 mm is cleaned and dried for later use;

[0127] (3) placing the raw material powder processed in step (1) and the backing tube processed in step (2) into a mold under vacuum and sealing them to form a composite structure with the backing tube in the center and the raw material layer around it, wherein the inner layer of the raw material layer has a particle size of 30 μm, the outer layer has a particle size of 80 μm, the inner layer has a thickness of 0.5 mm, and the outer layer has a thickness of 9.5 mm;

[0128] (4) After completing step (3), the raw material and the back tube composite structure are subjected to cold isostatic pressing to obtain a blank, the pressure is 210 MPa, and the holding time is 120 min;

[0129] (5) The blank obtained in step (4) is subjected to hot isostatic pressing to obtain a rotating target at a temperature of 0.8T. m (T m =890℃), pressure 30MPa, heat and pressure holding time 150min, during the cooling process, the cooling rate in the sintering furnace is controlled to be 5℃ / min (raw material layer cooling rate), and cooling water is introduced into the back tube. The cooling water flow rate is dynamically adjusted by the automatic temperature control device to control the back tube cooling rate. The back tube is controlled to be 200℃ lower than the raw material layer temperature, which is recorded as target B2.

[0130] Comparative Examples 16 to 20

[0131] The preparation method is basically the same as that in Example 4, and the differences are shown in Table 4. The obtained rotary targets are sequentially recorded as targets B6' to B10'.

[0132] Table 4 Process parameters of Example 2 and Comparative Examples 16 to 20

[0133]

[0134] Example 5

[0135] (1) Degassing Tb powder with a particle size of 30 μm and Tb powder with a particle size of 80 μm for standby use;

[0136] (2) The 304 stainless steel backing tube with an outer diameter of 90 mm is cleaned and dried for later use;

[0137] (3) placing the raw material powder processed in step (1) and the backing tube processed in step (2) into a mold under vacuum and sealing them to form a composite structure with the backing tube in the center and the raw material layer around it, wherein the inner layer of the raw material layer is a powder with a particle size of 30 μm, the outer layer is a powder with a particle size of 80 μm, the inner layer is 0.5 mm thick, and the outer layer is 9.5 mm thick;

[0138] (4) After completing step (3), the raw material and back tube composite structure are hot isostatically pressed to obtain a target material at a temperature of 0.8T. m (T m =1356°C), pressure 28MPa, holding time 150min, during the cooling process, the cooling rate in the sintering furnace is controlled to be 5°C / min (raw material layer cooling rate), and cooling water is introduced into the back tube. The cooling water flow rate is dynamically adjusted by the automatic temperature control device to control the back tube cooling rate. The back tube is controlled to be 100°C lower than the raw material layer temperature, which is recorded as target A3.

[0139] Comparative Examples 21 to 25

[0140] The preparation method is basically the same as that in Example 5, and the differences are shown in Table 5. The obtained rotary targets are sequentially recorded as target A11' to target A15'.

[0141] Table 5 Process parameters of Example 5 and Comparative Examples 21 to 25

[0142]

[0143] Example 6

[0144] (1) Degassing a DyFe alloy powder (Dy mass ratio 80%) with a particle size of 30 μm and a DyFe alloy powder with a particle size of 80 μm for standby use;

[0145] (2) The 304 stainless steel backing tube with an outer diameter of 90 mm is cleaned and dried for later use;

[0146] (3) placing the raw material powder processed in step (1) and the backing tube processed in step (2) into a mold under vacuum and sealing them to form a composite structure with the backing tube in the center and the raw material layer around it, wherein the inner layer of the raw material layer has a particle size of 30 μm, the outer layer has a particle size of 80 μm, the inner layer has a thickness of 0.5 mm, and the outer layer has a thickness of 9.5 mm;

[0147] (4) After completing step (3), the raw material and back tube composite structure are hot isostatically pressed to obtain a target material at a temperature of 0.8T. m (T m =890°C), pressure 26MPa, holding time 150min, during the cooling process, the cooling rate in the sintering furnace is controlled to be 5°C / min (raw material layer cooling rate), and cooling water is introduced into the back tube. The cooling water flow rate is dynamically adjusted by the automatic temperature control device to control the back tube cooling rate. The back tube is controlled to be 200°C lower than the raw material layer temperature, which is recorded as target B3.

[0148] Comparative Examples 26 to 30

[0149] The preparation method is basically the same as that in Example 6, and the differences are shown in Table 6. The obtained rotary targets are sequentially recorded as target B11' to target B15'.

[0150] Table 6 Process parameters of Example 6 and Comparative Examples 26 to 30

[0151]

[0152] Embodiments 7 to 12

[0153] Basically the same as Example 3, the differences are shown in Table 7, and the obtained rotary targets are A4, A5, B4, B5, C1, and C2 respectively.

[0154] Table 7 Parameter comparison of Examples 7 to 12

[0155]

[0156] Examples 13 to 18

[0157] Basically the same as Example 5, except for the differences shown in Table 8.

[0158] Table 8 Parameter comparison of Examples 13 to 18

[0159]

[0160]

[0161] Performance test of target material:

[0162] 1. Welding rate test

[0163] Test method: Use ultrasonic flaw detection equipment to detect the welding rate of target material.

[0164] The test results are shown in Table 9.

[0165] 2. Density test:

[0166] Test method: Use the drainage method to test the density of the target material.

[0167] See Table 8 for the test results.

[0168] 3. Test method for whether welding is performed during use

[0169] The magnetron sputtering was used for verification, and the target utilization rate of 70-80% without welding was used as the criterion for judging whether the target was welded.

[0170] Table 9 Performance parameters of various embodiments and comparative examples

[0171]

[0172]

[0173] It can be seen from Table 9 that the rotary target material provided by the embodiment of the present invention has better comprehensive performance when using material layers of different particle sizes and controlling the temperature difference between the back tube and the target tube during the cooling process:

[0174] (1) Whether it is cold pressing + pressureless sintering, or cold pressing + hot isostatic pressing, or direct hot isostatic pressing sintering, the density can reach more than 96%, and the highest can reach 99%, which meets the requirements of sputtering target materials. However, only when there is a difference in the particle size of the first and second layers of raw materials and there is a temperature difference between the back tube and the raw material (target tube) during the cooling process, the target material welding rate can reach more than 95%, and there is no problem of open welding, which meets the requirements of target material sputtering. The highest welding rate of Tb rotary target can reach 99.5%, the highest welding rate of DyFe alloy target can reach 98.5%, the highest welding rate of Dy target is 99.5%, and the highest welding rate of AlSc alloy target is 98%.

[0175] (2) Under the conditions of controlling the particle size of the first layer and the second layer of raw materials and controlling the temperature difference between the back tube and the target tube, cold pressing + pressureless sintering, or cold pressing + hot isostatic pressing sintering, or direct hot isostatic pressing sintering can all prepare rare earth rotating targets with a welding rate of more than 95%, a density of more than 96%, and no welding during use.

[0176] In summary, when the target material provided by the embodiment of the present invention is used for magnetron sputtering, the target material density is 96% to 99%, the welding rate is 95% to 99.5%, and there is no welding during the use process, which meets the application requirements in the fields of magnetic material coating grain boundary diffusion, storage and electronic information.

[0177] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a rare earth rotating target, characterized in that: include: Putting a backing tube and a powdered raw material into a mold to form a composite structure with the backing tube in the center and raw material layers around it, wherein the raw material includes a rare earth metal element and / or a rare earth alloy, and the raw material layers include a first raw material layer and a second raw material layer, the first raw material layer is located between the backing tube and the second raw material layer, and the raw material particle size in the first raw material layer is smaller than the raw material particle size in the second raw material layer; The composite structure is subjected to cold isostatic pressing or hot isostatic pressing to obtain a rare earth rotary target, wherein the cold isostatic pressing comprises cold isostatic pressing to obtain a blank and sintering the blank, and during the cooling process of the cold isostatic pressing and hot isostatic pressing, a certain temperature difference is maintained between the back tube and the raw material layer to obtain the rare earth rotary target; During the cooling process, the back tube and the raw material layer are controlled to maintain a certain temperature difference, specifically including: During the cooling process, control the temperature difference T between the back tube and the raw material layer X -T d =50~300℃, where T x T is the temperature of the one with smaller expansion coefficient between the back tube and the raw material layer, d It is the temperature of the one with the larger expansion coefficient between the back tube and the raw material layer.

2. The method for preparing a rare earth rotary target according to claim 1, characterized in that: The thickness of the first raw material layer is 0.1-1 mm, the particle size of the raw material in the first raw material layer is 1-100 μm, and the particle size of the raw material in the second raw material layer is 10-150 μm.

3. The method for preparing a rare earth rotary target according to claim 2, characterized in that: The particle size of the raw material in the second raw material layer is 2 to 3 times the particle size of the raw material in the first raw material layer.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The specific conditions of the cold isostatic pressing include: The pressure is 50-500MPa, and the holding time is 80-200min.

5. The preparation method according to any one of claims 1 to 3, characterized in that: The specific conditions for sintering the blank include: Pressureless sintering in vacuum or inert atmosphere; Sintering temperature T1 satisfies: When T 原料 ≤T 背管 When T1 = 0.5 ~ 0.95T 原料 ; When T 原料 >T 背管 When T1 = 0.5 ~ 0.95T 原料 , and T1<0.8T 背管 ; The sintering time is 30 to 250 minutes; Among them, T 原料 is the melting point of the raw material, T 背管 is the melting point of the back tube.

6. The preparation method according to any one of claims 1 to 3, characterized in that: The specific conditions for sintering the blank include: Perform hot isostatic pressing sintering; The sintering pressure is 5-50MPa; Sintering temperature T1 satisfies: When T 原料 ≤T 背管 When T1 = 0.5 ~ 0.9T 原料 ; When T 原料 >T 背管 When T1 = 0.5 ~ 0.9T 原料 , and T1<0.8T 背管 ; The sintering time is 30 to 240 minutes; Among them, T 原料 is the melting point of the raw material, T 背管 is the melting point of the back tube.

7. The preparation method according to any one of claims 1 to 3, characterized in that: The composite structure is subjected to hot isostatic pressing, specifically comprising: Performing hot isostatic pressing sintering on the composite structure; The sintering pressure is 10~60MPa; Sintering temperature T1 satisfies: When T 原料 ≤T 背管 When T1 = 0.5 ~ 0.9T 原料 ; When T 原料 >T 背管 When T1 = 0.5 ~ 0.9T 原料 , and T1<0.8T 背管 ; The sintering time is 30 to 270 minutes; Among them, T 原料 is the melting point of the raw material, T 背管 is the melting point of the back tube.

8. The rare earth rotary target prepared by the preparation method according to any one of claims 1 to 7.

9. Application of the rare earth rotating target prepared by the preparation method according to any one of claims 1 to 7 in the fields of magnetic material coating grain boundary diffusion, storage and electronic information.