A hemostatic hydrogel and its preparation method and application

By preparing oxidized sodium alginate hydrogel containing sea octopus, we solve the problems of complicated preparation of existing hemostatic materials and slow wound healing, achieve rapid hemostasis and promote wound healing, and provide efficient and low-cost hemostasis. Material.

CN115887745BActive Publication Date: 2024-10-11BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211476089.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2024-10-11
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Existing hemostatic materials are complex to prepare, have poor wound healing speed, poor absorption of wound tissue fluid, and high anticoagulant index.

Method used

A hemostatic hydrogel with a three-dimensional porous structure is prepared by using oxidized sodium alginate, an amino-containing polymer and sea clam powder. The hydrogel loaded with sea clams is formed through Schiff base reaction, providing an environment for rapid hemostasis and promoting wound healing. .

Benefits of technology

It achieves rapid hemostasis, low hemolysis rate, low anticoagulation index and high swelling rate, promotes wound healing, provides a moist environment to reduce wound temperature, has a wide range of applications and is low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115887745B_ABST
    Figure CN115887745B_ABST
Patent Text Reader

Abstract

The present invention provides a hemostatic hydrogel and a preparation method and application thereof, which relates to the field of materials, in order to solve the technical problems of complicated preparation of hemostatic materials and poor wound healing speed. The preparation method of the hemostatic hydrogel comprises the following steps: dissolving oxidized sodium alginate in water to form a first solution; dissolving an amino-containing polymer in water, adding cuttlebone powder to mix to form a second solution, wherein the proportion of cuttlebone in the second solution is 5wt / v% to 30wt / v%; mixing the first solution and the second solution to react to form a hydrogel, wherein the weight ratio of oxidized sodium alginate to the amino-containing polymer is (1 to 5): 1. The hemostatic hydrogel of the present invention has a short gelling time, a high swelling rate, can effectively absorb wound exudate, and the formed three-dimensional porous structure can successfully load cuttlebone, is simple and fast to operate, has high processing efficiency, low cost, and a wide range of applicability, and can quickly and efficiently prepare cuttlebone-loaded wound healing materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of materials, and in particular to a hemostatic hydrogel and a preparation method and application thereof. Background Art

[0002] The skin is one of the most important organs in the body, and it is a protective barrier against various external substances. In daily life, the skin is easily damaged by various external factors such as external force or surgery, which can cause the continuity of the skin epithelium or mucosal epithelial lining to be destroyed, forming wounds.

[0003] Using dressings to stop bleeding quickly and prevent secondary wound damage can promote wound healing and reduce trauma complications. In the prior art, dressing preparation is relatively complicated, dressings have poor absorption of wound tissue fluid, high anticoagulant index, and long wound healing time. Therefore, it is necessary to provide a hemostatic material that is conducive to rapid wound healing. Summary of the invention

[0004] The purpose of the present invention is to provide a hemostatic hydrogel and a preparation method and application thereof, so as to solve the technical problems of complex preparation of hemostatic materials and poor wound healing speed.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The embodiment of the present invention provides a method for preparing a hemostatic hydrogel, comprising the following steps:

[0007] dissolving oxidized sodium alginate in water to form a first solution;

[0008] Dissolving an amino-containing polymer in water, adding cuttlebone powder and mixing to form a second solution, wherein the cuttlebone accounts for 5 wt / v% to 30 wt / v% of the second solution;

[0009] The first solution and the second solution are mixed to react to form the hydrogel, wherein the weight ratio of the oxidized sodium alginate to the amino group-containing polymer is (1-5):1.

[0010] According to at least one embodiment of the present disclosure, the oxidation degree of the oxidized sodium alginate is 9% to 80%.

[0011] According to at least one embodiment of the present disclosure, the preparation method further comprises:

[0012] Sodium alginate and sodium periodate are reacted to generate the oxidized sodium alginate, and the weight ratio of the sodium alginate to the sodium periodate is 1:(0.2-2).

[0013] According to at least one embodiment of the present disclosure, sodium alginate is reacted with sodium periodate to generate the oxidized sodium alginate, and ethylene glycol is used to terminate the oxidation reaction. The weight ratio of the ethylene glycol to the sodium alginate is (5-10):1.

[0014] According to at least one embodiment of the present disclosure, the polymer containing an amino group includes one of gelatin, modified hyaluronic acid and chitosan.

[0015] According to at least one embodiment of the present disclosure, the modified hyaluronic acid is produced by grafting adipic acid diacylate onto hyaluronic acid through an amidation reaction.

[0016] According to at least one embodiment of the present disclosure, the particle size of the cuttlebone powder is 100 mesh to 500 mesh.

[0017] Compared with the prior art, the preparation method of the hemostatic hydrogel of the present invention uses a hydrophilic polymer containing an aldehyde group or a hydrophilic polymer with an aldehyde group in the polymer group through an oxidation reaction, oxidizes sodium alginate as one of the raw materials for preparing the hydrogel, uses a polymer containing an amino group or a polymer modified by amino as another raw material for preparing the hydrogel, and evenly disperses the sea cucumber powder in the polymer solution containing the amino group; the first solution and the second solution containing the two raw materials are mixed and then Schiff base reaction is performed to obtain a hydrogel loaded with sea cucumber. This hydrogel has a three-dimensional porous structure, can effectively absorb wound exudate, and has the advantages of short gel time, high swelling rate, good biocompatibility and blood compatibility. Among them, sea cucumber can regulate a variety of growth factors, promote collagen synthesis, and has the effects of hemostasis and coagulation, antibacterial and anti-inflammatory, enhancing immune function, and resisting lipid peroxidation. The hydrogel with a porous structure provided by the embodiment of the present invention not only has a short gel time, but also has a high swelling rate, and can effectively absorb wound exudate. At the same time, the hydrogel in the embodiment of the present invention has a high water content, which can provide a moist environment for the wound, reduce the temperature of the skin wound, and provide a moist environment for the wound to promote wound healing.

[0018] The three-dimensional porous structure of the hydrogel can successfully load the cuttlebone. It is not only simple and fast to operate, but also has high processing efficiency, low cost, and a wide range of applications. It can quickly and efficiently prepare wound healing materials loaded with cuttlebone. The hydrogel and cuttlebone work together. The cuttlebone can quickly stop bleeding and heal wounds. The hydrogel can provide a moist environment for the wound to further promote wound healing. The prepared hydrogel containing cuttlebone has a low hemolysis rate, a low anticoagulant index, can quickly stop bleeding, and can promote the proliferation and adhesion of fibroblasts, which is beneficial to wound healing.

[0019] Another object of the present invention is to provide a hemostatic hydrogel prepared by the above-mentioned method for preparing the hemostatic hydrogel.

[0020] Compared with the prior art, the hemostatic hydrogel of the present invention has the following advantages:

[0021] The advantages of the hemostatic hydrogel and the preparation method of the hemostatic hydrogel described above over the prior art are the same, and will not be described in detail herein.

[0022] Another object of the present invention is to provide a use of the hemostatic hydrogel in a dressing.

[0023] Compared with the prior art, the above application of the present invention has the following advantages:

[0024] The application of hemostatic hydrogel in dressing has the same advantages as the above-mentioned preparation method over the prior art, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings illustrate exemplary embodiments of the present disclosure and together with the description serve to explain the principles of the present disclosure. These drawings are included to provide a further understanding of the present disclosure and are incorporated in and constitute a part of this specification.

[0026] Figure 1 It is a schematic diagram of a process for preparing a hemostatic hydrogel according to an embodiment of the present disclosure.

[0027] Figure 2 is the gel time of oxidized sodium alginate / gelatin hydrogel at different oxidation degrees according to an embodiment of the present disclosure.

[0028] Figure 3 is a scanning electron microscope image of an oxidized sodium alginate / gelatin hydrogel with an oxidation degree of 79.93% according to an embodiment of the present disclosure.

[0029] Figure 4 is a scanning electron micrograph of the oxidized sodium alginate / gelatin hydrogel loaded with 15% cuttlebone according to Example 1.

[0030] Figure 5 It is a swelling ratio curve diagram of oxidized sodium alginate / gelatin hydrogel loaded with different contents of cuttlebone according to Examples 1, 4-7.

[0031] Figure 6 It is a graph of cell proliferation of oxidized sodium alginate / gelatin hydrogels loaded with different contents of cuttlebone according to Examples 1, 4-7.

[0032] Figure 7 It is a graph of the anticoagulation index of oxidized sodium alginate / gelatin hydrogels loaded with different contents of cuttlebone according to Examples 1, 4-7. DETAILED DESCRIPTION

[0033] The present disclosure is further described in detail below in conjunction with the accompanying drawings and implementations. It is understood that the specific implementations described herein are only used to explain the relevant content, rather than to limit the present disclosure. It should also be noted that, for ease of description, only the parts related to the present disclosure are shown in the accompanying drawings.

[0034] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present disclosure can be combined with each other. The present disclosure will be described in detail below with reference to the accompanying drawings and in conjunction with the embodiments. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0035] The single hydrogel in the prior art has poor mechanical properties, long gel time and poor hemostatic properties. Cuttlebone is the dried inner shell of the marine animal squid. Cuttlebone is rarely used to treat wounds and is mostly used for internal treatment of internal diseases. Even if it is used for external hemostasis, the wound heals slowly due to the lack of a moist environment.

[0036] For the preparation method of the oxidized sodium alginate / gelatin hydrogel loaded with cuttlebone provided in the embodiment of the present invention, please refer to Figure 1 As shown,

[0037] Step S100: dissolving oxidized sodium alginate in water to form a first solution, specifically dissolving a polymer containing an aldehyde group in deionized water, or aldehyde-forming a polymer without an aldehyde group and then dissolving it in deionized water, to obtain a raw material required for preparing a hydrogel. The present disclosure uses oxidized sodium alginate as an example for explanation, and it is understood that other aldehyde-containing polymers are suitable for the present preparation method;

[0038] Step S200: dissolving the polymer containing amino groups in water, adding cuttlebone powder and mixing to form a second solution, wherein the proportion of cuttlebone in the second solution is 5wt / v% to 30wt / v%; specifically, dissolving the polymer containing amino groups in deionized water, or aminated the polymer and dissolving it in deionized water, adding cuttlebone powder and mixing evenly after it is completely dissolved, to form a hydrogel raw material containing cuttlebone for standby use, wherein the proportion of cuttlebone in the second solution is exemplarily 7wt / v% to 27wt / v%, optionally 10wt / v% to 25wt / v%, and optionally 16wt / v% to 20wt / v%.

[0039] Step S300: Mix the first solution and the second solution to react to form a hydrogel, wherein the weight ratio of oxidized sodium alginate to the polymer containing an amino group is (1-5):1, exemplarily (2-4.5):1, optionally (2.5-4):1, and optionally (3.5-4):1. The two solutions are mixed evenly in proportion, and after standing for a period of time, a hydrogel is formed by a Schiff base reaction.

[0040] In the above preparation method, the hydrogel loaded with cuttlebone is obtained by mixing two solutions to undergo Schiff base reaction. The hydrogel has a short gel time, a high swelling rate, and can effectively absorb wound exudate. The formed three-dimensional porous structure can successfully load the cuttlebone. The operation is simple and fast, the processing efficiency is high, the cost is low, and the application range is wide. The cuttlebone-loaded wound healing material can be prepared quickly and efficiently. Cuttlebone is the dried inner shell of the marine animal squid. As a hemostatic and wound-healing drug, it can regulate multiple growth factors and promote collagen synthesis. The material is easy to obtain. By loading the cuttlebone in the three-dimensional porous structure of the hydrogel, the hydrogel not only provides a carrier for the cuttlebone, but also swells relatively large to absorb tissue fluid. At the same time, the water content can reach 70-90%, which can provide a moist environment for the wound and reduce the temperature of the skin wound. It is mainly used for dry chronic wounds, necrotic wounds, pressure sores and burn wounds, etc. The cuttlebone has a high coagulation ability in this moist environment and can quickly stop bleeding, which makes up for the poor hemostatic performance of the hydrogel. The interaction between the two promotes the proliferation of epidermal cells and promotes rapid wound healing.

[0041] See also Figure 3-Figure 4 As shown, Figure 3 The scanning electron micrograph of the oxidized sodium alginate / gelatin hydrogel with an oxidation degree of 79.93% is shown. Figure 4 The scanning electron micrograph of oxidized sodium alginate / gelatin hydrogel loaded with 15% cuttlebone is shown. By comparing the two, it can be seen that Figure 4 The three-dimensional porous structure in the porous skeleton is conducive to the transportation of oxygen and nutrients. The addition of cuttlebone makes the surface of the porous skeleton rough from the original smooth surface, which is conducive to the transportation of oxygen and nutrients. This rough structure is formed by the cuttlebone attached to the porous skeleton through hydrogen bonds and ionic bonds after being added to the gelatin / sodium alginate hydrogel.

[0042] For example, the oxidation degree of the above-mentioned oxidized sodium alginate is 9% to 80%, see Figure 2 As shown, Figure 2 10% oxidized sodium alginate and 10% gelatin with different oxidation degrees are shown in the figure, wherein the higher the oxidation degree of sodium alginate, the shorter the hydrogel gelation time. Therefore, sodium alginate with different oxidation degrees can be selected and prepared according to the required gelation time. The shortest hydrogel gelation time can be controlled at 100 seconds, thereby quickly gelling.

[0043] There are various methods for preparing oxidized sodium alginate. The present disclosure exemplifies the reaction of sodium alginate and sodium periodate to generate oxidized sodium alginate. The weight ratio of sodium alginate to sodium periodate is 1:(0.2-2), optionally 1:(0.4-1.7), optionally 1:(0.5-1.3), and optionally 1:(0.7-1). The feed ratio between the two can be selected according to different oxidation degrees. Sodium alginate is dissolved in an ethanol solvent to form a suspension, and sodium periodate is dissolved in deionized water. The two are mixed and reacted in the dark. The hydroxyl groups of the polymer are oxidized to aldehyde groups through an aldehyde reaction. Ethylene glycol is used to terminate the above oxidation reaction, wherein the weight ratio of ethylene glycol to sodium alginate is (5-10):1, optionally the weight ratio of ethylene glycol to sodium alginate is (6-8):1, and optionally the weight ratio of ethylene glycol to sodium alginate is (6.5-7.5):1. The addition of ethylene glycol also needs to be protected from light for a certain period of time to terminate the oxidation reaction.

[0044] Exemplarily, the above-mentioned polymer containing amino groups includes one of gelatin, modified hyaluronic acid and chitosan, and is not limited to the above three types, wherein the modified hyaluronic acid can be generated by grafting adipic acid diacyl to hyaluronic acid through an amidation reaction. Specifically, under the catalysis of 1-ethyl-3 (3-dimethylaminopropyl)-carbodiimide hydrochloride (abbreviated as EDC) and 1-hydroxybenzotriazole (abbreviated as HOBT), the carboxyl group of hyaluronic acid and the amino group of adipic acid dihydrazide (abbreviated as ADH) undergo an amidation reaction to graft ADH onto the hyaluronic acid molecular chain to obtain a polymer containing amino groups. In the process of forming the second solution, gelatin is dissolved at 50-60°C for 1-2h until the gelatin is completely dissolved.

[0045] In order to obtain a well-dispersed cuttlebone and further obtain a hydrogel with uniform distribution of cuttlebone, the particle size of the cuttlebone powder is 100-500 mesh. Specifically, the cuttlebone is washed with deionized water to remove surface impurities, placed in an oven to dry, and then ground and crushed, and then passed through a 100-500 mesh sieve, and the filtered cuttlebone powder is collected for use.

[0046] Several examples of preparation methods for hemostatic hydrogels are given below, and representative hemostatic hydrogels are selected for performance analysis.

[0047] Example 1

[0048] The preparation method of the hemostatic hydrogel provided in this embodiment specifically includes:

[0049] S1. Pretreatment of cuttlebone: Wash the cuttlebone with deionized water to remove surface impurities, dry it in an oven, grind it and pass it through a 200-mesh sieve, collect the filtered cuttlebone powder for later use;

[0050] S2. Preparation of oxidized sodium alginate: at room temperature, 5 g of sodium alginate was dissolved in 50 ml of ethanol to form a uniform suspension, 5.3 g of sodium periodate was dissolved in 50 ml of deionized water, the sodium alginate solution and the sodium periodate solution were mixed and reacted in the dark for 4 hours, and then 10 ml of ethylene glycol was added and reacted in the dark for 0.5 hour to terminate the oxidation reaction, the reaction product was dialyzed in deionized water with a 3500Da dialysis bag for 5 days, the dialyzed solution was collected and freeze-dried, and finally oxidized sodium alginate was obtained;

[0051] S3, preparation of the first solution: 0.5 g of oxidized sodium alginate is dissolved in deionized water to form a first solution with a concentration of 10% for later use;

[0052] S4, preparation of the second solution: 0.5 g of gelatin was placed in deionized water and heated at 55° C. for 1.5 h to form a solution with a concentration of 10%. After the gelatin was completely dissolved, 15 wt / v% of cuttlebone powder was added and mixed evenly to form a second solution containing cuttlebone;

[0053] S5. Synthesis of hydrogel: The first solution and the second solution are mixed in equal volumes to form a hydrogel through a Schiff base reaction. (Note: hydrogel + 15% of sea cucumber)

[0054] Example 2

[0055] The preparation method of the hemostatic hydrogel provided in this embodiment specifically includes:

[0056] S1. Pretreatment of cuttlebone: Wash the cuttlebone with deionized water to remove surface impurities, dry it in an oven, grind it and pass it through a 200-mesh sieve, collect the filtered cuttlebone powder for later use;

[0057] S2. Preparation of oxidized sodium alginate: at room temperature, 5 g of sodium alginate was dissolved in 50 ml of ethanol to form a uniform suspension, 5.3 g of sodium periodate was dissolved in 50 ml of deionized water, the sodium alginate solution and the sodium periodate solution were mixed and reacted in the dark for 4 hours, and then 10 ml of ethylene glycol was added and reacted in the dark for 0.5 hour to terminate the oxidation reaction, the reaction product was dialyzed in deionized water with a 3500Da dialysis bag for 5 days, the dialyzed solution was collected and freeze-dried, and finally oxidized sodium alginate was obtained;

[0058] S3. Modification of hyaluronic acid: at room temperature, 1 g of hyaluronic acid was dissolved in 200 ml of water, and 13 g of ADH was added after it was completely dissolved, and the pH was adjusted to 7.0 with sodium hydroxide. 1.56 g of EDC and 1.54 g of HOBT were completely dissolved in H2O / DMSO (10 ml / 10 ml) solvent and added to the hyaluronic acid solution, and then the pH of the solution was adjusted to 7.0 with 0.1 mol / L hydrochloric acid and 0.1 mol / L sodium hydroxide. After reacting for 12 hours, the reaction product was dialyzed in deionized water for 5 days with a 5000 Da dialysis bag, and the dialyzed solution was collected and freeze-dried to obtain modified hyaluronic acid;

[0059] S4, preparation of the first solution: 0.5 g of oxidized sodium alginate is dissolved in deionized water to form a first solution with a concentration of 10% for later use;

[0060] S5. Preparation of the second solution: at room temperature, 0.5 g of modified hyaluronic acid was dissolved in deionized water to form a solution with a concentration of 10%. After the hyaluronic acid was completely dissolved, 20 wt / v% of cuttlebone powder was added and mixed evenly to form a second solution containing cuttlebone;

[0061] S6. Synthesis of hydrogel: The first solution and the second solution are mixed in equal volumes to form a hydrogel through a Schiff base reaction.

[0062] Example 3

[0063] The preparation method of the hemostatic hydrogel provided in this embodiment specifically includes:

[0064] S1. Pretreatment of cuttlebone: Wash the cuttlebone with deionized water to remove surface impurities, dry it in an oven, grind it and pass it through a 200-mesh sieve, collect the filtered cuttlebone powder for later use;

[0065] S2. Preparation of oxidized sodium alginate: at room temperature, 5 g of sodium alginate was dissolved in 50 ml of ethanol to form a uniform suspension, 5.3 g of sodium periodate was dissolved in 50 ml of deionized water, the sodium alginate solution and the sodium periodate solution were mixed and reacted in the dark for 4 hours, and then 10 ml of ethylene glycol was added and reacted in the dark for 0.5 hour to terminate the oxidation reaction, the reaction product was dialyzed in deionized water with a 3500Da dialysis bag for 5 days, the dialyzed solution was collected and freeze-dried, and finally oxidized sodium alginate was obtained;

[0066] S3, preparation of the first solution: 0.5 g of oxidized sodium alginate is dissolved in deionized water to form a first solution with a concentration of 10% for later use;

[0067] S4, preparation of the second solution: at room temperature, 0.1 g of chitosan powder was placed in a 1% glacial acetic acid solution and stirred vigorously to obtain a 2% chitosan solution, after the chitosan was completely dissolved, 20 wt / v% of cuttlebone powder was added and mixed evenly to form a second solution containing cuttlebone;

[0068] S5. Synthesis of hydrogel: The first solution and the second solution are uniformly mixed in a volume ratio of 1:2 to form a hydrogel through a Schiff base reaction.

[0069] Example 4

[0070] The only difference between this embodiment and embodiment 1 is that in step S4, cuttlebone is not added.

[0071] (Note: hydrogel)

[0072] Example 5

[0073] The difference between this embodiment and embodiment 1 is that in step S4, 5 wt / v% of cuttlebone is added. (denoted as: hydrogel + cuttlebone 5%)

[0074] Example 6

[0075] The difference between this embodiment and embodiment 1 is that in step S4, 10 wt / v% of cuttlebone is added. (denoted as: hydrogel + cuttlebone 10%)

[0076] Example 7

[0077] The difference between this embodiment and embodiment 1 is that in step S4, 20 wt / v% of cuttlebone is added. (denoted as: hydrogel + 20% of cuttlebone)

[0078] Comparative Example 1

[0079] S1. Pretreatment of cuttlebone: Wash the cuttlebone with deionized water to remove surface impurities, dry it in an oven, grind it and pass it through a 200-mesh sieve, collect the filtered cuttlebone powder for later use;

[0080] S2. At room temperature, 0.1 g of chitosan powder was placed in a 1% glacial acetic acid solution and stirred vigorously to obtain a 2% chitosan solution. After the chitosan was completely dissolved, 20 wt / v% of cuttlebone powder was added and mixed evenly. The finished product was obtained after freeze-drying.

[0081] The hemolysis rates and coagulation times of the oxidized sodium alginate / gelatin hydrogels loaded with different contents of cuttlebone in Examples 1, 4-7 are given below, as shown in Tables 1 and 2.

[0082] Table 1 Hemolysis rate of hydrogel

[0083]

[0084] Table 2 Coagulation time of hydrogel

[0085]

[0086] See also Figure 5 As shown, Figure 5 The swelling ratio curves of the oxidized sodium alginate / gelatin hydrogels loaded with different contents of cuttlebone in Examples 1, 4-7 are shown. As the content of cuttlebone increases, the swelling ratio of the hydrogel increases first and then decreases. The maximum swelling ratio of the hydrogel loaded with 15% cuttlebone in Example 1 is between 11-12, which can effectively absorb the exudate from the wound. Please refer to Figure 6 As shown in Table 1, the oxidized sodium alginate / gelatin hydrogels loaded with different contents of cuttlebone in Examples 1, 5-7 can promote the adhesion and proliferation of fibroblasts, have good biocompatibility, and are beneficial to promoting wound healing. As shown in Table 1, the hemolysis rate of the hydrogels in Examples 1, 4-7 is much less than 5% and will not cause hemolysis reaction, and has blood compatibility.

[0087] See also Figure 7 As shown in Table 2, with the increase of the content of cuttlebone, the coagulation index of the hydrogel first decreases and then increases. The anticoagulation index of the hydrogel loaded with 15% cuttlebone in Example 1 is lower than 0.6, and the anticoagulation index and coagulation time are both lower than those of the hydrogel without cuttlebone in Example 4, indicating that the hydrogel loaded with cuttlebone has good in vitro coagulation performance and can stop bleeding quickly and effectively. And the hydrogel in Example 1 can quickly gel in about 100 seconds.

[0088] The hyaluronic acid / sodium alginate hydrogel loaded with cuttlebone prepared in Example 2 can quickly gel in 150 seconds, and the formed three-dimensional porous structure is conducive to the adhesion of cuttlebone, and the maximum swelling ratio is between 11-12, which can effectively absorb wound exudate. The hydrogel can promote the adhesion and proliferation of fibroblasts, has good biocompatibility, and is conducive to promoting wound healing. In addition, the hemolysis rate of the hydrogel is less than 5%, does not cause hemolytic reaction, has blood compatibility, the anticoagulation index is less than 0.6, has good in vitro coagulation performance, and coagulated blood clots appear on the surface of the hydrogel.

[0089] The chitosan / sodium alginate hydrogel loaded with cuttlebone prepared in Example 3 can quickly gel in about 130 seconds, with a maximum swelling ratio between 10-11, and can effectively absorb wound exudate. The hydrogel can promote the adhesion and proliferation of fibroblasts, has good biocompatibility, and is conducive to promoting wound healing. In addition, the hemolysis rate of the hydrogel is less than 5%, does not cause hemolytic reaction, has blood compatibility, and has an anticoagulant index of less than 0.6. It has good in vitro coagulation performance, and coagulated blood clots appear on the surface of the hydrogel. The anticoagulant index of the freeze-dried chitosan / cuttlebone material prepared in Comparative Example 1 is 0.85. Therefore, Example 3 of the present invention has better in vitro coagulation performance than Comparative Example 1. This is because the hydrogel in the embodiment of the present invention provides a certain moist environment, so that the hemostatic effect of the cuttlebone can be exerted, thereby promoting rapid healing of the wound.

[0090] As can be seen from the above, the hydrogel containing cuttlebone used in the embodiment of the present invention not only has a fast gelation speed, but also is simple to process and produce, and can quickly prepare a dressing loaded with cuttlebone for wound healing. Combining the two for synergistic effect not only has a lower hemolysis rate and a low anticoagulant index, but also can promote the proliferation and adhesion of fibroblasts.

[0091] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments / methods or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.

[0092] Those skilled in the art should understand that the above embodiments are only for the purpose of clearly illustrating the present disclosure, and are not intended to limit the scope of the present disclosure. For those skilled in the art, other changes or modifications may be made based on the above disclosure, and these changes or modifications are still within the scope of the present disclosure.

Claims

1. A method for preparing a hemostatic hydrogel, characterized in that: The following steps are involved: dissolving oxidized sodium alginate in water to form a first solution; Dissolving the polymer containing amino groups in water, adding cuttlebone powder and mixing to form a second solution, wherein the cuttlebone powder accounts for 15 wt / v% in the second solution; The first solution and the second solution are mixed to react to form the hydrogel, wherein the weight ratio of the oxidized sodium alginate to the amino group-containing polymer is (1-5):1; The oxidation degree of the oxidized sodium alginate is 80%; The amino group-containing polymer includes one of gelatin and chitosan.

2. The method for preparing the hemostatic hydrogel according to claim 1, characterized in that: The preparation method further comprises: Sodium alginate and sodium periodate are reacted to generate the oxidized sodium alginate, and the weight ratio of the sodium alginate to the sodium periodate is 1:(0.2-2).

3. The method for preparing the hemostatic hydrogel according to claim 2, characterized in that: The sodium alginate is reacted with sodium periodate to generate the oxidized sodium alginate, and ethylene glycol is used to terminate the oxidation reaction. The weight ratio of the ethylene glycol to the sodium alginate is (5-10):

1.

4. The method for preparing the hemostatic hydrogel according to claim 1, characterized in that: The particle size of the cuttlebone powder is 100-500 meshes.

5. A hemostatic hydrogel, characterized in that: The hemostatic hydrogel is prepared by the preparation method of any one of claims 1 to 4.