A dual laser additive manufacturing method and device
Through the dual-laser additive manufacturing method, the first laser is used to form an induced molten pool and the second laser is used to form a formed molten pool, and stirred in the formed molten pool, which solves the problems of molten pool temperature and material uniformity, and improves the quality of metal parts. performance.
Patent Information
- Application Number
- CN202211432201.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-16
AI Technical Summary
In laser selective melting technology, the generation of molten pool, solidification rate and temperature field uniformity have an important impact on the performance of metal parts. However, due to laser scattering and molten pool excitation leading to energy waste and unstable thermal factors, the existing technology It is difficult to effectively improve the temperature uniformity and material composition uniformity of the molten pool.
Using a dual-laser additive manufacturing method, the first laser forms a small-diameter induced molten pool, and the second laser forms a larger-diameter formed molten pool, and the driving device is used to cause the first laser to rapidly stir in the formed molten pool to improve melting. Temperature uniformity and material composition uniformity of the liquid phase inside the pool.
The absorption rate of the second laser is increased, energy waste is reduced, the temperature uniformity of the liquid phase inside the forming molten pool is enhanced, material segregation is weakened, and the performance of the final formed component is improved.
Smart Images

Figure CN115889820B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal 3D printing, and in particular to a dual-laser additive manufacturing method and device. Background Art
[0002] Metal 3D printing technology refers to a technology that uses digital model design as the basis, uses powdered metal or resin and other bondable materials to construct three-dimensional objects through layer-by-layer "additive" printing. Metal 3D printing technology has the advantages of high precision, short cycle, personalization, material diversity and low cost. Metal 3D printing technology includes laser selective melting technology, electron beam selective melting technology and laser engineering net forming technology. Among them, laser selective melting technology is an important part of the field of metal 3D printing.
[0003] Selective laser melting is abbreviated as SLM. In SLM technology, the laser spot quickly melts the metal powder on the powder bed of the forming platform, and then the laser spot scans according to the preset path, through point-by-point line, and then line-by-line to form a surface, through layer-by-layer printing, finally forming a complete metal part; in the laser printing process, the laser spot is focused on a point on the metal powder bed, forming a molten pool at this point. The depth and size of the molten pool are often much larger than the diameter of the laser spot, and the molten pool moves with the movement of the spot. Through the continuous generation of new molten pools and the solidification of old molten pools, the powder constituting the entity of the metal part is melted and solidified into a metal entity structure. Therefore, in the process of continuous formation and solidification of the molten pool, the generation of the molten pool, the solidification rate of the molten metal in the molten pool, and the uniformity of the temperature field of the molten metal in the molten pool have an important influence on the performance of the final parts, especially the generation of the molten pool. Due to the scattering of the laser and the moment of molten pool excitation, more energy waste will be caused, and more unstable thermal factors will be caused to the forming process. Summary of the invention
[0004] The present invention provides a dual-laser additive manufacturing method and device, which can more efficiently perform laser melting to manufacture metal parts.
[0005] To achieve the above object, the technical solution of the present invention is as follows:
[0006] A dual laser additive manufacturing method, comprising the following steps:
[0007] S1, a first laser emits a first laser, and a focused spot formed by the first laser forms an induced molten pool on a preset forming path;
[0008] S2, the second laser emits a second laser, and the focused spot formed by the second laser forms a forming molten pool on the induced molten pool, and the cross-sectional area of the forming molten pool is larger than the cross-sectional area of the induced molten pool;
[0009] S3. The driving device drives the first laser to stir rapidly in the forming molten pool to heat the liquid phase inside the forming molten pool.
[0010] Furthermore, an induced molten pool position is provided on the preset forming path, and a focused light spot formed by the first laser forms an induced molten pool at the induced molten pool position.
[0011] Furthermore, the focused spot formed by the second laser forms the forming molten pool with the induced molten pool as the center.
[0012] Furthermore, the first laser is a pulsed laser, and the diameter of the focused spot formed by the first laser is smaller than the diameter of the focused spot formed by the second laser.
[0013] Furthermore, the diameter of the focused spot formed by the first laser is 5-15 μm, and the diameter of the focused spot formed by the second laser is 40-60 μm.
[0014] Furthermore, the depth of the induced molten pool is greater than or equal to the depth of the formed molten pool.
[0015] Furthermore, the driving device drives the first laser to stir rapidly in the forming molten pool area through a beam reflecting mirror.
[0016] A dual-laser additive manufacturing device, comprising:
[0017] A first laser, wherein the first laser is used to emit a first laser, and a focused light spot formed by the first laser is used to form an induced molten pool in a preset forming path;
[0018] a second laser, the second laser being used to emit a second laser, the focused spot formed by the second laser being used to form a forming molten pool on the induced molten pool, the cross-sectional area of the forming molten pool being larger than the cross-sectional area of the induced molten pool;
[0019] A driving device is used to drive the first laser to quickly stir in the forming molten pool to heat the liquid phase inside the forming molten pool.
[0020] Furthermore, it also includes a calculation unit, which is used to determine the induced molten pool position on the preset forming path, and the first laser forms the induced molten pool at the induced molten pool position.
[0021] Furthermore, it also includes a galvanometer, and the first laser and the second laser share the galvanometer.
[0022] Furthermore, it also includes a beam reflector, and the driving device drives the beam reflector to enable the first laser to move quickly in the forming molten pool area.
[0023] Furthermore, the first laser is a pulsed laser, and a diameter of a focused spot formed by the first laser is smaller than a diameter of a focused spot formed by the second laser.
[0024] Furthermore, the diameter of the focused spot formed by the first laser is 5-15 μm, and the diameter of the spot formed by the second laser is 40-60 μm.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) In step S1 of the present invention, a first laser emits a first laser, which is reflected by a beam reflecting mirror and then transmitted through a beam reflecting lens to a forming platform, thereby forming an induced molten pool on the forming platform. In step S2, a second laser emits a second laser, which is reflected by a beam reflecting lens and then transmitted to an induced molten pool formed on the forming platform, thereby forming a forming molten pool on the forming platform. Before the second laser forms a forming laser, a high-energy small-spot laser is generated by the first laser at the center of the molten pool to be melted, thereby generating an induced molten pool. When the second laser moves by 5 mm or 2 s, the first laser forms an induced molten pool on the forming platform. The induced molten pool includes a variety of physical phase structures, and the height of the liquid level inside the induced molten pool is smaller than the height of the powder on the forming platform. After the second laser is incident on the induced molten pool in a larger range, the light scattered by the liquid phase and powder particles inside the induced molten pool moves in all directions, and the scattered light is absorbed by the powder to be melted, thereby improving the absorption rate of the second laser, facilitating the further formation of a forming molten pool by the second laser, and reducing the waste of the second laser energy.
[0027] (2) The beam reflector of the present invention is connected to a driving device, which can make the beam reflector rotate within a small range. Since the diameter of the focusing spot formed by the first laser is smaller than the diameter of the focusing spot formed by the second laser, the rotation of the beam reflector can make the first laser move within the range of the forming molten pool formed by the second laser. The second laser forms a forming molten pool on the forming platform. The first laser moves rapidly inside the forming molten pool formed by the second laser, rollingly heating the liquid phase inside the forming molten pool, thereby improving the temperature uniformity of the liquid phase inside the forming molten pool, reducing the material segregation inside the forming molten pool, and improving the performance of the final formed component. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the overall structure of the comparative document CN107096920B.
[0029] Figure 2 It is a schematic diagram of the overall structure of the comparative document CN111020569A.
[0030] Figure 3A three-dimensional diagram of a forming platform for inducing a molten pool state according to the present invention.
[0031] Figure 4 This is a schematic diagram of the movement path of the first laser inside the forming molten pool when the first laser is used as a stirring laser in the present invention.
[0032] Figure 5 The front view of the forming platform for inducing the molten pool state according to the present invention.
[0033] Figure 6 This is the front view of the forming platform when the second laser is irradiated to induce the molten pool according to the present invention.
[0034] Figure 7 It is a schematic diagram of the overall structure of the present invention.
[0035] Description of reference numerals:
[0036] 1. Second laser; 11. Second laser; 2. First laser; 21. First laser; 3. Collimating lens; 4. Beam reflecting mirror; 5. Beam reflecting lens; 6. Galvanometer; 7. Field lens; 8. Forming platform; 9. Inducing molten pool; 10. Driving device; 12. Stirring path; 13. Forming molten pool. DETAILED DESCRIPTION
[0037] The technical solution of the present invention will be clearly described below in conjunction with the accompanying drawings. Obviously, the described embodiments are not all embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention. It should be noted that the orientation or position relationship indicated by the terms "center", "up", "down", "left", "right", "vertical", "horizontal", etc. is based on the orientation or position relationship shown in the accompanying drawings. It is only for the convenience of describing the present invention and simplifying the description. It does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0038] like Figure 1As shown, the prior art CN107096920B discloses a non-average dual-beam synchronous scanning laser selective melting device and an optical path synthesis method. The non-average dual-beam synchronous scanning laser selective melting device includes a large spot laser beam incident device, a small spot laser beam incident device, a large spot beam reflector, a small spot beam reflector, an XY galvanometer scanning device and a field mirror. The incident outlets of the large spot laser beam incident device and the small spot laser beam incident device correspond to the large spot beam reflector and the small spot beam reflector respectively. The combined laser beam after the beam transmission through the mirror and the small spot beam reflector reaches the inside of the XY galvanometer scanning device, and finally enters the molding area through the field mirror. The distance between the field mirror and the molding plane of the molding area is equal to the focal length of the small spot laser beam, which can focus the small beam on the molding plane, while ensuring that the large spot laser beam is in a defocused state on the molding plane, so that the large spot laser beam can play the role of preheating the molding plane before it is melted, and provide a short temperature reduction gradient for the solidification process of the metal powder after melting, so as to achieve the purpose of temporary tempering.
[0039] like Figure 2 As shown, the prior art CN111020569A discloses a single-beam dual-spot composite energy field laser cladding head and its optical components, including a support frame, a channel for the laser beam to be injected is provided inside the support frame, a right prism semi-transparent beam reflector is also provided inside the support frame, the external laser injected from the upper part of the support frame is injected along the laser beam injection channel onto the right prism semi-transparent beam reflector, the right prism semi-transparent beam reflector is in a truncated cone shape, the upper bottom surface is arranged parallel to the lower bottom surface, the injected external laser is transmitted through the upper bottom surface and the lower bottom surface of the right prism semi-transparent beam reflector, a reflector and a conical reflector connected to the driving mechanism are also provided inside the support frame, the light spot transmitted from the upper bottom surface and the lower bottom surface of the right prism semi-transparent reflector is reflected by the conical reflector to the reflector connected to the driving device The mirror surface is reflected to the surface of the workpiece to form a stirring spot; the side of the right prism semi-transparent beam reflector is a reflecting surface, the outer spot of the aforementioned light spot is reflected out through the reflecting surface, and an annular reflector is arranged around the outer side of the right prism semi-transparent reflector, the reflecting surface of the annular reflector is parallel to the side of the right prism semi-transparent beam reflector, the light spot reflected from the side of the right prism semi-transparent reflector is reflected to the surface of the workpiece through the annular reflector, forming an annular spot for laser cladding; in the process of laser cladding additive manufacturing, while the large cladding spot is laser cladding, the stirring spot performs laser stirring on the molten pool that has not yet solidified, which is beneficial to avoid the generation of pores in the cladding process, and can also make the molten pool more uniform, the grains remelted and refined, and the cladding surface forming morphology smoother.
[0040] The present application proposes a dual-laser additive manufacturing method and device, the method comprising:
[0041] The first laser 1 emits a first laser 11, and the focused spot formed by the first laser 11 is used to form an induced molten pool 9 on a preset forming path; in the present application, the first laser 11 can be a pulsed laser, specifically a femtosecond pulsed laser, and the first laser 11 has the characteristics of a small spot and high energy. In the 3D printing forming process, the laser needs to melt the powder on the powder bed of the forming platform 8 according to a preset path. In the present application, the powder on the powder bed is irradiated by the first laser 11 to form an induced molten pool 9 on the powder bed, and the induced molten pool 9 has a high depth-to-diameter ratio.
[0042] In some optional embodiments, before the first laser 11 forms the induced molten pool 9, it is necessary to set an induction position on the 3D preset path, and then the first laser 11 irradiates the powder material at the position according to the coordinates of the position to form the induced molten pool 9. Specifically, in the present application, on the preset path of 3D printing, the position of the induced molten pool 9 is determined by setting the position coordinates. When the first laser 11 moves to the coordinate position of the induced molten pool 9 under the action of the galvanometer 6, the first laser 1 is turned on and excites the first laser 11, and the first laser 11 forms the induced molten pool 9 with the position coordinates as the center. In the present application, the setting of the position of the induced molten pool 9 can be set according to actual needs. For example, when the 3D printing path running interval is 5mm, the first laser 1 can excite the first laser 11 once to form an induced molten pool 9, or when the path scan is at a time interval of 2s, the first laser 11 is excited to form an induced molten pool 9. It should be understood that the above-mentioned position setting of the induced molten pool 9 is only an example setting, and of course, the induced molten pool 9 can be set at each position point of the path scanning.
[0043] In some optional embodiments, the diameter of the focused spot formed by the first laser 11 emitted by the first laser 1 is 5-15 microns.
[0044] The second laser 2 emits a second laser 21 , and the focused spot formed by the second laser 21 is used to form a forming molten pool 13 on the induced molten pool 9 , and the cross-sectional area of the forming molten pool 13 is larger than the cross-sectional area of the induced molten pool 9 .
[0045] The focused spot formed by the second laser 21 forms a forming molten pool 13 on the induced molten pool 9, where the forming molten pool 13 can also be called a scanning molten pool or a processing molten pool. By moving the processing molten pool, the formed molten pool solidifies, thereby forming a solid part structure. In the present application, the center of the focused spot formed by the second laser 21 is located in the central area of the induced molten pool 9, and the processing molten pool is formed on the basis of the induced molten pool 9. The second laser 21 can be a continuous laser, and the diameter of its spot is larger than that of the first laser 11. Its spot energy distribution can be a Gaussian distribution or a flat-top distribution. The second laser 21 forms a larger processing molten pool on the basis of the induced molten pool 9. That is to say, when the second laser 21 starts to scan and form a processing molten pool, the induced molten pool 9 forms a whole with the processing molten pool, and at this time the first laser 11 is no longer used to form the induced molten pool 9.
[0046] In some optional embodiments, the depth of the induced molten pool 9 is greater than or equal to the depth of the formed molten pool 13. When the induced molten pool 9 forms a deeper molten pool, its deep hole structure is very conducive to the metal powder particles absorbing the energy of the second laser 21.
[0047] In some optional embodiments, the diameter of the focused spot formed by the second laser 21 emitted by the second laser 2 is 40-60 μm.
[0048] The driving device 10 drives the first laser 11 to stir rapidly in the forming molten pool 13 to heat the liquid phase inside the forming molten pool 13 .
[0049] In the present application, the first laser 11 and the second laser 21 form a coaxial beam after passing through the beam reflector 5 and the beam reflector lens 4, and then the coaxial laser beam is formed under the action of the optical components such as the galvanometer 6 and the field lens 7, and then acts on the forming platform 8. The driving device 10 drives the first laser 11 beam to stir rapidly in the forming molten pool 13. Specifically, the driving device 10 can drive the beam reflector 5 to move rapidly at a small angle, thereby driving the first laser 11 to change the reflection angle rapidly within a small range, so that under the action of the galvanometer 6, in addition to following the coaxial movement of the second laser 21, it can also move rapidly within the small range of the coaxial axis. This movement can quickly heat the liquid in the forming molten pool 13 formed by the second laser 21 in turn, so that the liquid phase in the molten pool can obtain a more uniform temperature field. This uniform temperature field can make the material components in the molten pool more uniform, which is conducive to improving the performance of the formed component.
[0050] It should be understood that in the present application, after the first laser 11 generates the induced laser and the second laser 21 forms the forming molten pool 13, the first laser 11 is transformed into a stirring spot under the action of the driving device 10, and the stirring spot moves rapidly along a preset path in the area of the forming molten pool 13 under the driving action of the driving device 10 on the beam reflector 5, thereby auxiliary heating the liquid phase in the forming molten pool 13. In some embodiments, the motion trajectory of the stirring spot can be a serpentine route or a circular route, which is not limited in the present application.
[0051] It should also be understood that the various steps of the dual laser additive manufacturing method proposed in this application only have a logical sequence relationship, and the order described in this application cannot be used as the order of operations in the actual implementation process. Technical personnel in this field should develop the process method in accordance with the logical sequence in the actual setting based on the core concept proposed in this application.
[0052] Combine the following Figure 3-Figure 7 The dual laser additive manufacturing method and device of the present application are described in detail.
[0053] The present invention provides a dual-laser additive manufacturing method, comprising the following steps:
[0054] S1, setting a plurality of induced molten pool 9 positions on a preset path, and predetermining a plurality of induced molten pool 9 positions on a preset forming path by a calculation unit;
[0055] S2, the first laser 1 emits a first laser 11. After being emitted from the inside of the first laser 1, the first laser 11 passes through the collimating lens 3 and then is emitted to the reflecting surface of the beam reflecting mirror 5. The first laser 11 is reflected by the beam reflecting mirror 5, and then passes through the galvanometer 6 and the field lens 7 to be emitted to the initial position to be scanned on the forming platform 8, so that an induced molten pool 9 is formed at the initial position to be scanned;
[0056] S3, the second laser 2 emits a second laser 21. After being emitted from the second laser 2, the second laser 21 passes through the collimating lens 3 and then is emitted to the reflecting surface of the beam reflecting lens 4. The second laser 21 is reflected by the beam reflecting lens 4, and then passes through the galvanometer 6 and the field lens 7 to be emitted to the induced molten pool 9 formed on the forming platform 8. The second laser 21 forms a forming molten pool 13 on the forming platform 8 while centering on the induced molten pool 9.
[0057] S4, start the driving device 10 to rotate the beam reflector 5, so that the first laser 11 moves within the spot diameter range of the second laser 21, and the spot of the first laser 11 moves quickly within the forming molten pool 13 formed by the second laser 21 to heat the liquid phase inside the forming molten pool 13;
[0058] S5, when the second laser 21 moves along a predetermined route, the first laser 11 moves synchronously with the path of the second laser 21;
[0059] S6. When the second laser 21 moves along the predetermined route every time it moves 5 mm or every time the second laser 21 moves 2 s, the first laser 11 induces the generation of the molten pool 9.
[0060] S7, repeat steps S2-S6 until the parts are processed.
[0061] Specifically, if Figure 3 As shown, before starting the melting scan of the second laser 21, the first laser 1 is firstly made to emit the first laser 11 to excite the molten pool at the initial position to be scanned, so as to form an induced molten pool 9. The induced molten pool 9 is within the range of the forming molten pool 13 formed by the subsequent second laser 21. The induced molten pool 9 can increase the absorption rate of the powder to the second laser 21 and improve the melting effect of the powder. The induced molten pool 9 formed by the first laser 11 on the powder bed can have the same depth as the forming molten pool 13. After the induced molten pool 9 is formed, the second laser 21 scans the forming molten pool 13 with the induced molten pool 9 as the center, and then the second laser 21 melts and forms the powder according to the preset path.
[0062] Every time the scanning path of the second laser 21 moves 5 mm, the first laser 11 induces the generation of the molten pool 9, or every time the second laser 21 moves 2 s, the first laser 11 induces the generation of the molten pool 9. In this way, multiple induced molten pools 9 can be formed in the entire path, which is beneficial to improving the absorption rate of the powder on the forming platform 8 to the second laser 21 and improving the melting effect of the powder.
[0063] like Figure 4 As shown, after the first laser 11 forms the induced molten pool 9 and the second laser 21 forms the formed molten pool 13, the first laser 11 becomes a stirring laser, and the driving device 10 drives the beam reflector 5 to make the first laser 11 move rapidly within the spot diameter range of the second laser 21, and stir rapidly inside the formed molten pool 13, so as to achieve a uniform temperature inside the formed molten pool 13. At this time, the motion trajectory of the first laser 11 can be serpentine, annular, etc. Figure 5 This is just a schematic diagram of the serpentine route and does not represent the only route.
[0064] like Figure 5 As shown, the forming platform 8 is in powder form, and the induced molten pool 9 forms a tiny area on the forming platform 8. The induced molten pool 9 includes a molten liquid phase, unmelted powder particles and semi-molten particles. These complex phase components increase the spectral absorption effect of the second laser 21, thereby being able to well induce the second laser 21 to form a larger molten pool.
[0065] The principle of inducing the molten pool 9 to increase the absorption of the second laser 21 in the present invention is as follows: Figure 6 As shown, the formed induced molten pool 9 contains liquid phase, unmelted powder particles, etc. The melted liquid phase makes the liquid level height lower than the powder height of the powder spread in the powder bed. When the second laser 21 is incident on the induced molten pool 9 in a larger range, the light scattered by the liquid phase and powder particles in the molten pool will move in all directions, rather than just being scattered in the forming space perpendicular to the powder bed height. The scattered light will be absorbed by the powder to be melted, thereby improving the laser absorption rate and reducing the waste of energy of the scanning laser, i.e., the second laser 21.
[0066] like Figure 7 As shown, the present invention also provides a dual-laser additive manufacturing device, including a second laser 2, a first laser 1, a collimating lens 3, a beam reflecting mirror 5, a beam reflecting lens 4, a galvanometer 6 and a field lens 7, the second laser 2 and the first laser 1 are arranged at the upper left end, the first laser 1 is located on the upper part of the second laser 2, the collimating lens 3 and the beam reflecting lens 4 are horizontally arranged in sequence on the right side of the second laser 2, and the collimating lens 3 and the beam reflecting mirror 5 are horizontally arranged in sequence on the right side of the first laser 1, the beam reflecting mirror 5 and the beam reflecting lens 4 are both arranged at an angle of 45° relative to the horizontal direction, and the reflecting surface of the beam reflecting lens 4 is arranged downward, the galvanometer 6 is arranged directly below the beam reflecting lens 4, and the field lens 7 is arranged below the galvanometer 6, and the forming platform 8 is directly below the field lens 7, there is a certain distance between the field lens 7 and the forming platform 8, and the projections of the beam reflecting mirror 5, the beam reflecting lens 4, the galvanometer 6, the field lens 7 and the forming platform 8 in the vertical direction overlap; and also includes a calculation unit, the calculation unit is used to determine the position of the induced molten pool 9 on the preset forming path.
[0067] The first laser 1 excites the first laser 11, which is a pulsed laser. The first laser 11 has the characteristics of small spot and concentrated energy. The focus spot diameter formed by the first laser 11 is 5-15μm. After the first laser 11 is emitted from the inside of the first laser 1, it passes through the collimating lens 3 arranged horizontally with the first laser 1, and then it is emitted to the reflection surface of the beam reflector 5. After the first laser 11 is reflected by the beam reflector 5, the path of the first laser 11 is transformed from horizontal to right to vertical downward; the second laser 2 excites the second laser 21, which is a scanning laser. The focus spot diameter formed by the second laser 21 is 40-60μm. The second laser 21 is emitted from the inside of the second laser 2, passes through the collimating lens 3 arranged horizontally with the second laser 2, and then is emitted to the reflection surface of the beam reflector lens 4 for reflection. Since the beam reflector lens 4 is located directly below the beam reflector 5, the first laser 11 is reflected and then passes through the beam reflector lens 4 to form a coaxial beam with the second laser 21. They enter the galvanometer 6 together, and then act on the powder area on the surface of the forming platform 8 through the field lens 7. The first laser 11 and the second laser 21 act on the powder bed through the same galvanometer 6 and field lens 7, so that the scanning speeds of the first laser 11 and the second laser 21 can be the same, and the synchronous scanning movement is maintained during the scanning process. The second laser 21 has a larger spot diameter, which is used to form a forming molten pool 13 on the powder bed of the forming platform 8. The molten pool is a tiny melting and solidification interval formed by the heat source acting on the powder in the powder bed 3D printing process. The area of the molten pool is generally 1.2-5 times the area of the scanning spot acting on the powder bed. The scanning spot belongs to a Gaussian distribution. The higher the energy is near the center of the spot, the lower the energy is away from the center. Therefore, although a larger liquid phase area is formed inside the molten pool, the temperature distribution in the liquid phase area inside the molten pool is seriously uneven, which affects the distribution of material components in the molten pool. Moreover, it will also cause greater stress during the solidification process, which is not conducive to the performance of the component formed after the molten pool solidifies.
[0068] A driving device 10 is arranged on the beam reflector 5. The driving device 10 is a driving motor. The driving motor can control the tilt angle of the beam reflector 5. The driving device 10 can drive the beam reflector 5 to rotate rapidly within a small range, so that the first laser 11 can change rapidly within a small range. The first laser 11 can also form coaxial light with the second laser 21 through the beam reflecting lens 4. The focus spot diameter formed by the second laser 21 is larger than the focus spot diameter formed by the first laser 11. The first laser 11 changes within the focus spot diameter range formed by the second laser 21, so that the first laser 11 and the second laser 21 remain coaxial to form nested spots of different sizes. The second laser 21 forms a forming molten pool 13 on the powder bed of the forming platform 8. Under the driving action of the beam reflector 5, the first laser 11 can move rapidly in the forming molten pool 13 to equalize and stir the liquid phase in the forming molten pool 13, thereby reducing the segregation of the material components inside the forming molten pool 13.
[0069] It should be understood that in the embodiments of the present application, Figure 7 The arrangement of the second laser 2 and the first laser 1 is only a schematic representation, and there can be a variety of actual construction methods. The driving device 10 can also control the beam reflecting lens 4. At this time, the second laser 21 emitted by the second laser 2 is a laser for forming an induced molten pool 9, and the first laser 11 emitted by the first laser 1 forms a formed molten pool 13; there can also be a variety of ways for the second laser 21 and the first laser 11 to form a coaxial light beam through the beam reflecting lens 4 and the beam reflecting mirror 5, and the schematic diagram of this embodiment is only one of them.
[0070] The above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, a person skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A dual laser additive manufacturing method, characterized in that: The following steps are involved: S1, a first laser emits a first laser, and a focused spot formed by the first laser forms an induced molten pool on a preset forming path; S2, the second laser emits a second laser, and the focused spot formed by the second laser forms a forming molten pool on the induced molten pool, and the cross-sectional area of the forming molten pool is larger than the cross-sectional area of the induced molten pool; S3, a driving device drives the first laser to rapidly stir in the forming molten pool to heat the liquid phase inside the forming molten pool; The induced molten pool includes a molten liquid phase, unmelted powder particles and semi-molten powder particles. When the second laser is incident on the induced molten pool in a larger range, the scattered light of the molten liquid phase and powder particles in the induced molten pool will move in all directions to be absorbed by the powder particles that need to be melted.
2. A dual laser additive manufacturing method according to claim 1, characterized in that: An induced molten pool position is set on the preset forming path, and the focused light spot formed by the first laser forms an induced molten pool at the induced molten pool position.
3. A dual laser additive manufacturing method according to claim 2, characterized in that: The focused spot formed by the second laser forms the forming molten pool with the induced molten pool as the center.
4. The dual laser additive manufacturing method according to claim 1, characterized in that: The first laser is a pulsed laser, and a diameter of a focused light spot formed by the first laser is smaller than a diameter of a focused light spot formed by the second laser.
5. A dual laser additive manufacturing method according to claim 4, characterized in that: The diameter of the focused light spot formed by the first laser is 5-15 μm, and the diameter of the focused light spot formed by the second laser is 40-60 μm.
6. The dual laser additive manufacturing method according to claim 1, characterized in that: The depth of the induced molten pool is greater than or equal to the depth of the formed molten pool.
7. The dual laser additive manufacturing method according to claim 1, characterized in that: The driving device drives the first laser to stir rapidly in the forming molten pool area through a beam reflecting mirror.
8. A dual laser additive manufacturing device, characterized in that: include: A first laser, wherein the first laser is used to emit a first laser, and a focused light spot formed by the first laser is used to form an induced molten pool in a preset forming path; a second laser, the second laser being used to emit a second laser, the focused spot formed by the second laser being used to form a forming molten pool on the induced molten pool, the cross-sectional area of the forming molten pool being larger than the cross-sectional area of the induced molten pool; A driving device, the driving device is used to drive the first laser to quickly stir in the forming molten pool to heat the liquid phase inside the forming molten pool; The induced molten pool includes a molten liquid phase, unmelted powder particles and semi-molten powder particles. When the second laser is incident on the induced molten pool in a larger range, the scattered light of the molten liquid phase and powder particles in the induced molten pool will move in all directions to be absorbed by the powder particles that need to be melted.
9. The dual laser additive manufacturing device according to claim 8, characterized in that: The method further comprises a calculation unit, wherein the calculation unit is used to determine an induced molten pool position on a preset forming path, and the first laser forms an induced molten pool at the induced molten pool position.
10. The dual laser additive manufacturing device according to claim 8, characterized in that: The invention also includes a galvanometer mirror, and the first laser and the second laser share the galvanometer mirror.
11. The dual laser additive manufacturing device according to claim 8, characterized in that: It also includes a beam reflecting mirror, and the driving device drives the beam reflecting mirror to enable the first laser to move quickly in the forming molten pool area.
12. The dual laser additive manufacturing device according to claim 8, characterized in that: The first laser is a pulsed laser, and a diameter of a focused light spot formed by the first laser is smaller than a diameter of a focused light spot formed by the second laser.
13. The dual laser additive manufacturing device according to claim 12, characterized in that: The diameter of the focused light spot formed by the first laser is 5-15 μm, and the diameter of the light spot formed by the second laser is 40-60 μm.
Citation Information
Patent Citations
Non-homogeneous dual-beam synchronous scanning laser selective melting apparatus and optical path synthesis method
CN107096920B
Single-beam double-light-spot composite-energy-field laser cladding head and optical assembly thereof
CN111020569A
Method of laser-welding metal materials by double lasers
CN103753022A
Device and method for refining structure crystalline grains in metal additive manufacturing process
CN110802229A
Dual-wavelength metal 3D printing light path device and 3D printing system
CN112605401A