A secondary particle artificial graphite negative electrode material and preparation method thereof

By using a composite of starch and asphalt or resin binders and the negative electrode raw material for pelletization and then direct graphitization, the existing process complexity and narrow application range problems are solved, and the material performance is improved and the cost is reduced. .

CN115893401BActive Publication Date: 2024-10-11LANZHOU GRIFFIN CARBON MATERIAL CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202211442652.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-17
Publication Date
2024-10-11
Estimated Expiration
2042-11-17

AI Technical Summary

Technical Problem

The existing anode material preparation process is complex and not suitable for new graphitization methods, such as box furnaces and continuous furnaces, which limits the improvement of the material's rate and cycle performance.

Method used

A composite of starch and asphalt or resin binders is mixed with the negative electrode raw material. After pelletization, it is directly graphitized to reduce the granulation process and is suitable for traditional and new graphitization furnaces.

Benefits of technology

It reduces the production cost, improves the rate and cycle performance of the material, increases the density and air permeability of the furnace, and expands the scope of application of the graphitization method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003947946720000071
    Figure BDA0003947946720000071
  • Figure BDA0003947946720000081
    Figure BDA0003947946720000081
  • Figure BDA0003947946720000082
    Figure BDA0003947946720000082
Patent Text Reader

Abstract

The present application relates to the field of preparation of negative electrode materials, and specifically to a secondary particle artificial graphite negative electrode material and a preparation method thereof, the preparation method comprising the following steps: the negative electrode raw material and the binder are mixed evenly, and then water is added and stirred to obtain a wet material, and the wet material is pelletized to obtain a spherical mixture; wherein the binder is a composite of a starch binder and an asphalt binder or a resin binder; the spherical mixture is heat-treated to obtain a dry and hardened pellet, and then graphitized; the graphitized pellet is crushed and screened to obtain a secondary particle artificial graphite negative electrode material. The binder and the negative electrode raw material powder are mixed and then pelletized and graphitized. After graphitization, the pellet still has some materials bonded. After crushing, breaking up and screening, a secondary particle artificial graphite negative electrode product is obtained. Compared with the traditional production process, the granulation process is reduced, the production cost can be greatly reduced, and the rate and cycle performance of the material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of negative electrode material preparation, and in particular to a secondary particle artificial graphite negative electrode material and a preparation method thereof. Background Art

[0002] Artificial graphite has significant advantages such as cycle performance, high rate charge and discharge efficiency and good electrolyte compatibility, and is currently the mainstream negative electrode material. With the explosive growth of the power and energy storage market, the market has put forward new demands for artificial graphite with better rate performance, longer life and lower cost. In order to improve the rate and cycle performance of the material, granulation is an important process link. The secondary particles formed after granulation can not only increase the lithium insertion points and improve the rate performance, but also reduce the expansion of the pole piece and extend the service life. In order to reduce costs, new graphitization methods such as box furnaces and continuous furnaces are gradually maturing and becoming mainstream. The new graphitization puts forward new requirements for the pre-process of raw materials, such as good air permeability and high bulk density, while traditional pre-processes such as crushing and granulation cannot meet these new process requirements well.

[0003] The traditional granulation process is to mechanically stir and heat the single particle raw material and solid or liquid binder in a reactor to complete the construction of a single particle into a multiple particle structure. For example, Chinese patent CN109956471A provides a process for granulating graphite negative electrode materials. This method puts the carbon source powder into the reactor for stirring and heating, and then sprays the liquid binder or coating agent onto the surface of the stirring powder for granulation, which improves the processing performance and use performance of the negative electrode product in the later stage. However, this method is complex and is only applicable to traditional Acheson furnace graphitization, and cannot be linked with new graphitization methods such as box furnaces and continuous furnaces. Summary of the invention

[0004] The main purpose of the present application is to provide a secondary particle artificial graphite negative electrode material and a preparation method thereof, aiming to solve the technical problems that the preparation of existing negative electrode materials requires granulation, the preparation steps are complicated, and the applicable methods for subsequent graphitization are narrow.

[0005] To achieve the above-mentioned purpose, the present application proposes a method for preparing a secondary particle artificial graphite negative electrode material, comprising the following steps: uniformly mixing the negative electrode raw material and the binder, adding water and stirring to obtain a wet material, and pelletizing the wet material to obtain a spherical mixture; wherein the binder is a composite of a starch binder and an asphalt binder or a resin binder;

[0006] heat treating the spherical mixture to obtain dried and hardened pellets, and then graphitizing the pellets;

[0007] The graphitized pellets are crushed and screened to obtain the secondary particle artificial graphite negative electrode material.

[0008] The binder used in this scheme is a mixture of a starch binder and an asphalt binder, or a mixture of a starch binder and a resin binder. The above binder has a bonding effect on the negative electrode raw material powder before and after graphitization, so that part of the material is still bonded in the finished product obtained at high temperature, so the obtained product is a secondary particle negative electrode product.

[0009] The traditional preparation process is to mix the material and the binder, stir them in a reactor at about 600°C, and then graphitize them to obtain a secondary particle negative electrode product; this solution directly mixes the material and the binder, spheroidizes them, and then puts them into a graphitization furnace for graphitization to obtain a secondary granulated product, which reduces the traditional granulation process and reduces the cost; at the same time, in addition to using the traditional Acheson furnace for graphitization, box furnaces, continuous graphitization furnaces, etc. can also be used for graphitization, which has a wider range of applications.

[0010] In this scheme, the negative electrode raw material and the binder are mixed evenly by physical means, such as VC, stirring, ball milling, wheel milling and other mixing methods. After the negative electrode material and the binder are mixed evenly, water is added to obtain a wet material. The wet material is more conducive to the subsequent formation of pellets. The water and the mixed material are also mixed physically, such as spraying, stirring, ball milling, and wheel milling. After that, the wet material is pelletized by mechanical force to extrude or spin-form the wet material. The equipment for pelletization can be a molding machine, a ball press, a strip extruder, a kneading machine, a pill making machine, a ball forming machine, etc. The obtained pellets can be pellets of a single shape or size, or a mixture of pellets of multiple shapes or sizes; the pellets can be specifically a block with a weight of 0-20kg, a sphere or ellipsoid with a diameter of 3-50m, or a strip or rhombus with a diameter of 3-50mm. Finally, the obtained pellets are graphitized and then crushed to obtain secondary particle artificial graphite negative electrode materials.

[0011] Preferably, the starch binder is natural water-soluble starch; the asphalt binder is water-soluble asphalt; and the resin binder is water-soluble resin. The binders used in this solution are all water-soluble binders, which can be directly dissolved in water, which is conducive to the subsequent pelletization process and can make the secondary particle artificial graphite negative electrode material have better performance.

[0012] Preferably, the natural water-soluble starch is at least one of corn starch, wheat starch, potato starch, sweet potato starch, gelatinized starch, oxidized starch, and esterified starch; the water-soluble asphalt is sulfonated asphalt;

[0013] The water-soluble resin is at least one of water-based polyurethane resin, water-based acrylic resin, water-based alkyd resin, water-based epoxy resin, and water-based polyester resin. When the above specific binder is used, the product performance improvement effect is the best.

[0014] Preferably, the weight ratio of the starch binder to the asphalt binder or the resin binder is 3-5:3-6. By adjusting the amount of the starch binder and the asphalt binder or the resin binder, the formed binder can adapt to various negative electrode raw materials and graphitization conditions, and has a wider range of adaptability.

[0015] Preferably, the mass ratio of the binder to the negative electrode raw material is 100:(5-30). In this solution, the amount of binder used is relatively small, and the quality of the secondary particle artificial graphite negative electrode material obtained is relatively good.

[0016] Preferably, the pellets after heat treatment have a volatile matter content of less than 3% and a moisture content of less than 2%; the heat treatment step is natural air drying or heating drying. Heat treatment of the pellets can remove moisture and volatile matter inside the pellets to obtain dry and hardened pellets. In addition to natural air drying, other heat treatment methods can use equipment such as ovens, drying kilns, and rotary kilns.

[0017] Preferably, the temperature during heating and drying is 90-150° C., or 700-1200° C. During heating and drying, the secondary particle artificial graphite negative electrode material has better performance.

[0018] Preferably, the negative electrode raw material is a crushed material obtained by crushing at least one of petroleum coke, pitch coke, needle coke, mesophase carbon microspheres, coal, and natural graphite. The negative electrode raw material may be carbonized or not.

[0019] Preferably, the particle size of the negative electrode raw material is 5-18 μm, and the volatile matter is 0-14%. Limiting the negative electrode raw material to the above conditions can ensure the quality of the pellets produced and better meet product requirements.

[0020] Preferably, when water is added and stirred, the mass ratio of the total mass of the mixture of the negative electrode raw material and the binder to the mass of the water is 100:(10-40).

[0021] In addition, the present invention also discloses a secondary particle artificial graphite negative electrode material, which is prepared by any of the above-mentioned methods for preparing the secondary particle artificial graphite negative electrode material.

[0022] The preparation method of the secondary particle artificial graphite negative electrode material of the present application has the following beneficial effects: the present solution directly mixes the binder and the negative electrode raw material powder and then performs pelletization and graphitization treatment. After graphitization, some materials in the pellets are still bonded together, and after crushing, breaking up and screening, a secondary particle artificial graphite negative electrode product is obtained. Compared with the traditional production process, the granulation process is reduced, the production cost can be greatly reduced, and the rate and cycle performance of the material are improved. In addition, the negative electrode raw material powder is extruded through pelletization treatment, which can increase the density of the pellets, increase the furnace loading capacity, and improve the air permeability, which is conducive to the overflow of volatile gases and greatly reduces the safety hazards in the new graphitization operation process. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0024] The present application proposes a method for preparing a secondary particle artificial graphite negative electrode material, comprising the following steps:

[0025] The negative electrode raw material and the binder are mixed evenly, and then water is added and stirred to obtain a wet material, and the wet material is pelletized to obtain a spherical mixture; wherein the binder is a composite of a starch binder and an asphalt binder or a resin binder;

[0026] The mass ratio of the binder to the negative electrode raw material is 100:(5-30); the weight ratio of the starch binder to the asphalt or the resin is 3-5:3-6; the mass ratio of the mixture of the negative electrode raw material and the binder to the water is 100:(10-40);

[0027] The starch binder is natural water-soluble starch; the asphalt binder is water-soluble asphalt; the resin binder is water-soluble resin;

[0028] The natural water-soluble starch is at least one of corn starch, wheat starch, potato starch, sweet potato starch, gelatinized starch, oxidized starch, and esterified starch;

[0029] The water-soluble asphalt is sulfonated asphalt;

[0030] The water-soluble resin is at least one of a water-based polyurethane resin, a water-based acrylic resin, a water-based alkyd resin, a water-based epoxy resin, and a water-based polyester resin;

[0031] The negative electrode raw material is a crushed material obtained by crushing at least one of petroleum coke, pitch coke, needle coke, mesophase carbon microspheres, coal, and natural graphite; the particle size of the negative electrode raw material is 5-18 μm, and the volatile matter is 0-14%;

[0032] Heat-treating the spherical mixture to obtain dried and hardened pellets, and then graphitizing the pellets; wherein the heat-treating step is natural air-drying or heat-drying, and the pellets after heat-treatment have a volatile matter of less than 3% and a moisture content of less than 2%; heating to 90-150° C. during heat-drying; or, heating to 700-1200° C. during heat-drying;

[0033] The graphitized pellets are crushed and screened to obtain the secondary particle artificial graphite negative electrode material.

[0034] The technical solution of the present application is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present application and are not used to limit the present application.

[0035] Example 1

[0036] A method for preparing a secondary particle artificial graphite negative electrode material comprises the following steps:

[0037] Potato starch and sulfonated asphalt are prepared in a mass ratio of 3:5 to obtain a binder;

[0038] The asphalt coke single particle carbonized material and the above-mentioned binder are mixed evenly at a weight ratio of 100:5; the particle size of the asphalt petroleum coke single particle uncarbonized material is 10 μm, and the volatile matter is 6%;

[0039] Add water to the mixed material and stir it evenly with a wheel mill to obtain a wet material, wherein the mass ratio of the mixture of the negative electrode raw material and the binder to water is 100:15, and then place the wet material in a molding machine for pelletization to obtain a spherical mixture;

[0040] The spherical mixture is placed in an oven and heat-treated at 150° C. to obtain dry and hardened pellets.

[0041] The pellets are graphitized in a box furnace, and the graphitized pellets are crushed and screened to obtain the secondary particle artificial graphite negative electrode material.

[0042] Example 2

[0043] A method for preparing a secondary particle artificial graphite negative electrode material comprises the following steps:

[0044] Sweet potato starch, esterified starch and sulfonated asphalt are prepared in a mass ratio of 2:1:2 (starch binder: asphalt binder = 3:2) to obtain a binder;

[0045] The needle coke single particle carbonized material and the above binder are uniformly mixed in a weight ratio of 100:10; the needle coke single particle carbonized material has a particle size of 20 μm and a volatile matter of 15%;

[0046] Add water to the mixed material and use a sprayer to spray and stir evenly to obtain a wet material, wherein the mass ratio of the mixture of the negative electrode raw material and the binder to water is 100:20, and then place the wet material in a ball press for pelletization to obtain a spherical mixture;

[0047] The spherical mixture is placed in a box furnace and heat treated at 1000°C to obtain dried and hardened pellets.

[0048] The pellets are graphitized using an Acheson furnace, and the graphitized pellets are crushed and screened to obtain the secondary particle artificial graphite negative electrode material.

[0049] Example 3

[0050] A method for preparing a secondary particle artificial graphite negative electrode material comprises the following steps:

[0051] The esterified starch and the water-based acrylic resin are prepared in a mass ratio of 4:5 to obtain a binder;

[0052] The uncarbonized single-particle petroleum coke material and the above-mentioned binder are mixed uniformly in a weight ratio of 100:15 using a VC machine; the particle size of the uncarbonized single-particle petroleum coke material is 9 μm, and the volatile matter is 10%;

[0053] Add water to the mixed material and stir it evenly with a wheel mill to obtain a wet material, wherein the mass ratio of the mixture of the negative electrode raw material and the binder to water is 100:30 to obtain a wet material, and then place the wet material in a ball press for pelletization to obtain a spherical mixture;

[0054] The spherical mixture is placed in a box furnace and heat treated at 700° C. to obtain dried and hardened pellets.

[0055] The pellets are graphitized in a continuous graphitization furnace, and the graphitized pellets are crushed and screened to obtain the secondary particle artificial graphite negative electrode material.

[0056] Example 4

[0057] A method for preparing a secondary particle artificial graphite negative electrode material comprises the following steps:

[0058] The gelatinized starch, water-based alkyd resin and water-based polyester resin are prepared in a mass ratio of 4:3:3 (starch binder: resin binder = 4:6) to obtain a binder;

[0059] The petroleum coke single particle carbonized material and the above-mentioned binder are mixed uniformly by a VC machine at a weight ratio of 100:15; the particle size of the petroleum coke single particle carbonized material is 13 μm, and the volatile matter is 10%;

[0060] Add water to the mixed material and stir it evenly with a wheel mill to obtain a wet material, wherein the mass ratio of the mixture of the negative electrode raw material and the binder to water is 100:30 to obtain a wet material, and then place the wet material in a ball press for pelletization to obtain a spherical mixture;

[0061] The spherical mixture is naturally air-dried at a temperature of 25-35° C. (heat treatment) to obtain dry and hardened pellets.

[0062] The pellets are graphitized in a box furnace, and the graphitized pellets are crushed and screened to obtain the secondary particle artificial graphite negative electrode material.

[0063] Comparative Example 1

[0064] The conditions in this comparative example are the same as those in Example 1, except that this comparative example uses a single starch binder, potato starch, mixed with the asphalt coke single particle carbonized material.

[0065] Comparative Example 2

[0066] The conditions in this comparative example are the same as those in Example 1, except that this comparative example uses a single asphalt binder - sulfonated asphalt mixed with asphalt coke single particle carbonized material.

[0067] Comparative Example 3

[0068] The conditions in this comparative example are the same as those in Example 3, except that this comparative example uses a single resin binder, water-based acrylic resin, mixed with a single particle of uncarbonized petroleum coke.

[0069] Comparative Example 4

[0070] The conditions in this comparative example are the same as those in Example 3, except that: this comparative example uses a combination of esterified starch and polyvinyl alcohol to form a binder, which is then mixed with the uncarbonized material of a single particle of petroleum coke.

[0071] The performance of the products obtained in Examples 1-4 and Comparative Examples 1-4 was tested, and the specific test results are shown in the following table:

[0072]

[0073] It can be seen from the test data in the above table that when the method of the present invention is used in the graphitization process, the furnace density is significantly improved, and the gaps between the pellets are conducive to the permeability of the material and the overflow of volatiles; the molding ratio of the negative electrode product after graphitization using the method of the present invention is increased, the specific surface area is smaller, and the granulation process is reduced, but the raw material powder also achieves the granulation effect, which greatly reduces the production cost.

[0074] Example 5

[0075] The conditions in this example are the same as those in Example 4, except that the drying conditions are: placing the spherical mixture in an oven and drying it at 100°C.

[0076] Example 6

[0077] The conditions in this example are the same as those in Example 4, except that the drying conditions are: placing the spherical mixture in a box furnace and drying it at 1000°C.

[0078] The performance of the products obtained in Examples 5-6 was tested, and the specific test results are shown in the following table:

[0079]

[0080] From the test data in the above table, it can be seen that compared with Example 4, the bonding effect of Example 5 and Example 6 is better, the charging density during graphitization is reduced, and the molding ratio of pellets after graphitization is increased. When the drying temperature is increased to 700-1200°C, the performance of the product is better.

[0081] Example 7

[0082] The conditions in this embodiment are the same as those in Embodiment 2, except that the particle size of the uncarbonized single particle of petroleum coke is 10 μm, and the volatile matter is 9% (the particle size in Embodiment 2 is 20 μm, and the volatile matter is 15%).

[0083] The product obtained in Example 7 was tested for performance, and the specific test results are shown in the following table:

[0084]

[0085] Compared with Example 2, the particle size and volatile matter of the negative electrode raw material used in Example 7 are reduced, which is beneficial to improving the rate and cycle performance of the material.

[0086] Example 8

[0087] The conditions in this embodiment are the same as those in embodiment 7, except that the binder in this embodiment is changed to a binder composed of corn starch, esterified starch and sulfonated asphalt. The mass ratio is the same as that in embodiment 7.

[0088] Example 9

[0089] The conditions in this embodiment are the same as those in embodiment 3, except that the binder in this embodiment is changed, and the mass ratio of the binder is also kept the same, and the specific adjustments are shown in the following table:

[0090] Binder raw materials Example 9-1 Corn starch and waterborne polyurethane resin Example 9-2 Corn starch and waterborne epoxy resin

[0091] The performance of the products obtained in Example 8 and Example 9 was tested, and the specific test results are shown in the following table:

[0092]

[0093] It can be seen from the test data in the above table that, compared with Example 7 and Example 3, Example 8, Example 9-1 and Example 9-2 are all preferred binders, which have better bonding effect, can increase the furnace density during graphitization, reduce the graphitization cost, and better ensure the quality of the negative electrode product; after graphitization, the pellet forming ratio increases, and the pellets are crushed and screened, which not only achieves the granulation effect, but also improves the rate and cycle performance of the material.

[0094] Example 10

[0095] The conditions in this example are the same as those in Example 8, except that the mass ratio of corn starch, esterified starch and sulfonated asphalt is adjusted from 2:1:2 to 2:1:5 (starch binder: asphalt binder = 3:5).

[0096] Embodiment 11

[0097] The conditions in this example are the same as those in Example 8, except that the mass ratio of corn starch, esterified starch and sulfonated asphalt is adjusted from 2:1:2 to 2:2:6 (starch binder: asphalt binder = 4:6).

[0098] The performance of the products obtained in Examples 10-11 was tested, and the specific test results are shown in the following table:

[0099]

[0100] It can be seen from the test data in the above table that compared with Example 8, after Examples 10-11 were adjusted to the preferred mass ratio, the charging density during the graphitization process was improved, and the molding ratio after graphitization was increased, indicating that increasing the mass ratio of the composite binder can enhance the bonding effect of the composite binder, so that the negative electrode raw material can achieve the granulation effect.

[0101] The above description is only a preferred embodiment of the present application, and does not limit the patent scope of the present application. All equivalent structural transformations made using the contents of the present application specification under the inventive concept of the present application, or direct / indirect application in other related technical fields are included in the patent protection scope of the present application.

Claims

1. A method for preparing a secondary particle artificial graphite negative electrode material, characterized in that: The following steps are involved: The negative electrode raw material and the binder are mixed evenly, and then water is added and stirred to obtain a wet material, and the wet material is pelletized to obtain a spherical mixture; wherein corn starch, esterified starch and sulfonated asphalt are prepared in a mass ratio of 2:2:6 to obtain the binder; the negative electrode raw material is a single-particle uncarbonized material of petroleum coke, and the single-particle uncarbonized material of petroleum coke and the binder are mixed evenly in a weight ratio of 100:10; the particle size of the single-particle uncarbonized material of petroleum coke is 10 μm, and the volatile matter is 9%; wherein water is added to the mixed material by a sprayer and stirred evenly to obtain the wet material, the mass ratio of the mixture of the negative electrode raw material and the binder to water is 100:20, and the wet material is pelletized by a ball press; Heat treating the spherical mixture in a box furnace at 1000° C. to obtain dry and hardened pellets, and then graphitizing the pellets in an Acheson furnace; The graphitized pellets are crushed and screened to obtain the secondary particle artificial graphite negative electrode material.

2. A secondary particle artificial graphite negative electrode material, characterized in that: The secondary particle artificial graphite negative electrode material is prepared by the preparation method of the secondary particle artificial graphite negative electrode material according to claim 1.

Citation Information

Cited By

  • Low-expansion and high-compaction-density artificial graphite material and preparation method thereof

    CN121850665A

  • A low-expansion, high-density artificial graphite material and a method for producing the same

    CN121850665B

  • Continuous secondary granulation process and system for artificial graphite negative electrode material

    CN121988224A