A method for recovering graphite from waste cathode carbon blocks in aluminum electrolysis

By combining low melting point inorganic salt roasting and mechanical activation, the energy consumption and pollution problems in the recycling of aluminum electrolysis waste cathode carbon block graphite are solved, green recycling and safe treatment of cyanide/fluorine toxic components are achieved, which is efficient and environmentally friendly , the characteristics of simple process.

CN115893404BActive Publication Date: 2024-10-25GUIZHOU NORMAL UNIVERSITY

Patent Information

Application Number
CN202310142389.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-21
Publication Date
2024-10-25
Estimated Expiration
2043-02-21

AI Technical Summary

Technical Problem

The existing graphite recycling method for waste cathode carbon blocks in aluminum electrolysis has problems such as high energy consumption, high carbon emissions, high pollution risks, and complex processes. It is difficult to achieve green recycling and safe dissociation of cyanide/fluorine toxic components.

Method used

Low-melting point inorganic salts are used for molten salt roasting, combined with mechanical activation and acidic solution leaching treatment, and the recycling and regeneration process of flue gas and acidic leachate is designed to achieve efficient recovery of graphite and safe treatment of cyanide/fluorine toxic components.

Benefits of technology

It realizes the recovery of high-quality graphite resources from aluminum electrolysis waste cathode carbon blocks, reduces energy consumption and carbon emissions, avoids environmental pollution, and has the characteristics of high efficiency, environmental protection, and simple process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of comprehensive utilization of solid waste resources from aluminum electrolysis, and specifically relates to a method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis. The method comprises the following steps: using a low-melting-point inorganic salt to carry out molten salt roasting treatment on the waste cathode carbon blocks from aluminum electrolysis to obtain roasted materials and flue gas; placing the roasted materials and an acidic solution in a mechanical activation device for leaching; carrying out solid-liquid separation after the reaction to obtain an acidic leaching solution and residual solid materials; then washing and drying the residual solid materials in sequence to obtain graphite and a washing solution; and simultaneously designing a recycling process for by-products such as flue gas and acidic leaching solution to avoid environmental pollution caused by waste gas and waste liquid, thereby realizing green recycling of high-quality graphite resources from waste cathode carbon blocks from aluminum electrolysis, safe dissociation of cyanide / fluorine toxic components, and regeneration and recycling of molten salt roasting agents. The method has the characteristics of high efficiency, environmental protection, and simple process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of comprehensive utilization of aluminum electrolysis solid waste resources, and specifically to a method for recovering graphite from aluminum electrolysis waste cathode carbon blocks. Background Art

[0002] At present, there are mainly the following methods for recovering graphite from waste cathode carbon blocks in aluminum electrolysis:

[0003] The first method is oxygen-isolated roasting, which mainly involves adding aluminum electrolysis waste cathode carbon blocks that have been crushed to a certain particle size into various high-temperature equipment for roasting under oxygen-isolated conditions. Low-melting-point inorganic salts such as sodium fluoride and cryolite contained in the graphite matrix will be separated in gaseous form, thereby realizing the recovery of graphite in the waste cathode carbon blocks. The disadvantage is that maintaining oxygen-isolated roasting requires a lot of energy and will bring about a large amount of carbon emissions. At the same time, gaseous fluorides will cause serious corrosion to the lining of high-temperature equipment, and the precipitation of metallic sodium will also increase the processing risk.

[0004] The second method is wet leaching, which mainly utilizes the solubility characteristics of inorganic salt components contained in waste cathode carbon blocks from aluminum electrolysis, screens water, alkali, acid or salt to form a single-stage or multi-stage solution system, and then leaches the waste cathode carbon block powder from aluminum electrolysis that has been crushed to a certain fineness to achieve effective separation and recovery of graphite powder. Its disadvantages are that reaction agents such as strong acids and strong alkalis have low safety, the treatment process is complicated, the leaching wastewater treatment is difficult, and it is easy to cause secondary pollution.

[0005] The third method is froth flotation, which mainly utilizes the difference in surface physical properties of graphite and inorganic salt components contained in waste cathode carbon blocks of aluminum electrolysis, and realizes foaming, activation, capture and pH adjustment of the slurry system through a combination of flotation agents, so as to promote the hydrophobic graphite powder to adhere to the bubbles and float up for recovery. Its disadvantage is that the fixed carbon content of the recovered graphite is relatively low, which is not conducive to the deep resource application of the recovered products. At the same time, the residual cryolite and sodium fluoride and other fluorine-containing components still have environmental pollution risks.

[0006] The fourth method is the alkali fusion method, which mainly uses a mechanical crushing method to break the waste cathode carbon blocks of aluminum electrolysis into powder, and then mixes them with alkaline agents such as sodium hydroxide and sodium carbonate, and then places the mixture in a high-temperature device for roasting. Finally, the graphite powder is recovered through aqueous solution leaching combined with solid-liquid separation. The disadvantage is that the alkali fusion treatment requires maintaining a high reaction temperature and a long reaction time, which is prone to generate a large amount of energy consumption and carbon emissions, and the cost of alkali fusion agents is high, and the recycling process is relatively complicated. Summary of the invention

[0007] In order to solve the problems existing in the prior art, the main purpose of the present invention is to propose a method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis, so as to realize the green recovery of high-quality graphite resources from waste cathode carbon blocks from aluminum electrolysis, the safe dissociation of cyanide / fluorine toxic components, and the regeneration and recycling of molten salt roasting agents, which has the characteristics of high efficiency, environmental protection and simple process.

[0008] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0009] A method for recovering graphite from waste cathode carbon blocks in aluminum electrolysis, comprising the following steps:

[0010] S1. Molten salt roasting

[0011] The waste cathode carbon blocks of aluminum electrolysis are subjected to molten salt roasting treatment using low melting point inorganic salt to obtain roasting materials and flue gas;

[0012] S2. Mechanical Activation

[0013] The calcined material and the acid solution are placed in a mechanical activation device for leaching. After the reaction is completed, solid-liquid separation is performed to obtain an acidic leaching solution and residual solid material. The residual solid material is then washed and dried in sequence to obtain graphite and a washing solution.

[0014] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis according to the present invention, the method further comprises:

[0015] S0. Preprocessing

[0016] The aluminum electrolysis waste cathode carbon blocks are refined, screened and dried to obtain aluminum electrolysis waste cathode carbon blocks with a particle size of ≤5mm.

[0017] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis according to the present invention, the method further comprises:

[0018] S3. Recycling of by-products

[0019] The flue gas generated in step S1 is introduced into the acidic leaching solution generated in step S2, and seed addition, vacuum concentration, cooling crystallization, solid-liquid separation, and freeze drying are performed in sequence to obtain low-melting-point inorganic salts and supernatant, which are returned to the molten salt roasting step and the mechanical activation step for water washing processes for recycling.

[0020] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis described in the present invention, wherein: in the step S1, the waste cathode carbon blocks from aluminum electrolysis are mechanically mixed with a low-melting-point inorganic salt in a mass ratio of 1:1 to 3 to obtain a mixed material; the mixed material is loaded into a graphite crucible and placed in a heating device, and then molten salt roasted in an air atmosphere at a roasting temperature of 100 to 250°C and a roasting time of 0.5 to 2.0 hours to obtain a roasted material and flue gas.

[0021] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis described in the present invention, in step S1, the low melting point inorganic salt is one or more of ammonium fluoride, ammonium bifluoride, and sodium bifluoride.

[0022] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis described in the present invention, wherein: in the step S2, the time of mechanical activation leaching is 0.1 to 1.0 h, and the rotation speed of the mechanical activation equipment is 500 to 700 r / min.

[0023] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis described in the present invention, in step S2, the acidic solution is one or more of hydrochloric acid, sulfuric acid, nitric acid, and perchloric acid.

[0024] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis described in the present invention, in step S2, the concentration of the acidic solution is 0.5-12 mol / L, and the liquid-to-solid ratio of the acidic solution to the roasted material is 5-20 mL / g.

[0025] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis described in the present invention, in step S2, the fixed carbon content of the graphite is ≥99.0%, and the water washing liquid is circulated for water washing treatment.

[0026] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis described in the present invention, in step S3, before adding seed crystals, the flue gas produced in step S1 is introduced into the acidic leaching solution produced in step S2 to adjust the pH value to 3-6.

[0027] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis described in the present invention, in step S3, the seed crystal is one or more of ammonium fluoride, ammonium bifluoride, and sodium bifluoride.

[0028] The beneficial effects of the present invention are as follows:

[0029] The present invention proposes a method for recovering graphite in waste cathode carbon blocks from aluminum electrolysis, which comprises the following steps: using low-melting-point inorganic salts to carry out molten salt roasting treatment on waste cathode carbon blocks from aluminum electrolysis to obtain roasted materials and flue gas, placing the roasted materials and acidic solution in mechanical activation equipment for leaching, and performing solid-liquid separation after the reaction to obtain acidic leaching liquid and residual solid materials, and then washing and drying the residual solid materials in sequence to obtain graphite and washing liquid; at the same time, a recycling process for by-products such as flue gas and acidic leaching liquid is designed to avoid environmental pollution caused by waste gas and waste liquid, thereby realizing green recycling of high-quality graphite resources of waste cathode carbon blocks from aluminum electrolysis, safe dissociation of cyanide / fluorine toxic components, and regeneration and recycling of molten salt roasting agents, and the method has the characteristics of high efficiency, environmental protection, and simple process. DETAILED DESCRIPTION

[0030] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] First, the present invention uses low-melting-point inorganic salts with significant mineral phase reconstruction ability to carry out molten salt roasting treatment on aluminum electrolysis waste cathode carbon blocks: on the one hand, the melting points of ammonium fluoride, ammonium bifluoride, and sodium bifluoride are only 95°C, 124.6°C, and 160°C, respectively, which can effectively control the molten salt roasting temperature below 250°C, which can not only greatly reduce energy consumption, but also shorten the heating / cooling time to improve the processing efficiency, and can promote the molten salt roasting process to be carried out in an air atmosphere, while avoiding the consumption of carbonaceous materials in the waste cathode carbon blocks, the oxidative decomposition of cyanide is achieved, and the decomposition rate of cyanide is ≥99.5%. On the other hand, the low-melting-point inorganic salt will melt and decompose during the molten salt roasting process to form a gas-solid-liquid three-phase reaction system, which can not only effectively convert the insoluble complex aluminum silicate into a water-soluble inorganic salt, but also has good applicability to particles with a particle size of 3 to 5 mm, thereby overcoming the technical difficulties of low particle size of graphite recovery in the existing technology, which is conducive to broadening the scope of resource utilization of recovered graphite.

[0032] Secondly, the present invention directly uses mechanical activation equipment to perform acid purification on the roasted material: on the one hand, mechanical activation with high stirring intensity and stirring uniformity replaces the traditional magnetic / mechanical stirring, which can not only significantly improve the contact degree between the roasted material and the acid solution, but also increase the reaction activity of the roasted material; at the same time, the soluble fluoride salt contained in the roasted material and the hydrogen ions introduced by the acid solution are used to construct HF-H +The mixed acid system significantly enhances the reactivity of the acidic solution, further promoting the efficient separation of graphite and inorganic salt components, with the fixed carbon content of the recovered graphite ≥99.0% and the leaching rate of fluoride ≥99.0%. On the other hand, compared with the traditional mechanical activation → wet leaching process, by coupling mechanical activation with acid leaching, the heat generated during the mechanical activation process can be used to supply acid leaching, shortening the process while improving the processing efficiency, and saving the processing cost and equipment investment of the wet leaching process.

[0033] Finally, the present invention innovatively designs the comprehensive utilization of roasting flue gas and the recycling of low-melting-point inorganic salts: on the one hand, the roasting flue gas rich in ammonia and fluorine-containing gas is passed into the acidic leaching solution, which can not only adjust the pH value with alkaline ammonia, but also enrich the fluorine-containing gas, thereby fully utilizing the resource properties of the roasting flue gas while avoiding the environmental pollution of the waste gas. On the other hand, by coupling the processes of pH adjustment, seed addition, vacuum concentration, cooling crystallization, solid-liquid separation, freeze drying, etc., the recycling of low-melting-point inorganic salts is achieved, with a recovery rate of ≥85%, effectively reducing the processing cost of waste cathode carbon blocks and avoiding secondary pollution of waste liquid.

[0034] According to one aspect of the present invention, the present invention provides the following technical solution:

[0035] A method for recovering graphite from waste cathode carbon blocks in aluminum electrolysis, comprising the following steps:

[0036] S1. Molten salt roasting

[0037] The waste cathode carbon blocks of aluminum electrolysis are subjected to molten salt roasting treatment using low melting point inorganic salt to obtain roasting materials and flue gas;

[0038] S2. Mechanical Activation

[0039] The calcined material and the acid solution are placed in a mechanical activation device for leaching. After the reaction is completed, solid-liquid separation is performed to obtain an acidic leaching solution and residual solid material. The residual solid material is then washed and dried in sequence to obtain graphite and a washing solution.

[0040] Preferably, before step S1, the step further includes:

[0041] S0. Preprocessing

[0042] The waste cathode carbon blocks from aluminum electrolysis are refined, screened and dried to obtain waste cathode carbon blocks from aluminum electrolysis with a particle size of ≤5 mm. Specifically, the particle size of the waste cathode carbon blocks from aluminum electrolysis can be, for example but not limited to, any one of ≤5 mm, ≤4 mm, ≤3 mm, ≤2 mm, ≤1 mm, ≤0.5 mm, ≤0.3 mm, and ≤0.15 mm.

[0043] Preferably, the step S2 further includes:

[0044] S3. Recycling of by-products

[0045] The flue gas generated in step S1 is introduced into the acidic leaching solution generated in step S2, and seed addition, vacuum concentration, cooling crystallization, solid-liquid separation, and freeze drying are performed in sequence to obtain low-melting-point inorganic salts and supernatant, which are returned to the molten salt roasting step and the mechanical activation step for water washing processes for recycling.

[0046] Preferably, in step S1, the waste cathode carbon blocks from aluminum electrolysis are mechanically mixed with low-melting-point inorganic salts in a mass ratio of 1:1 to 3 to obtain a mixed material; the mixed material is loaded into a graphite crucible and placed in a heating device, and then molten salt is roasted in an air atmosphere at a roasting temperature of 100 to 250°C and a roasting time of 0.5 to 2.0 hours to obtain a roasted material and flue gas; the low-melting-point inorganic salt is one or more of ammonium fluoride, ammonium bifluoride, and sodium bifluoride. Specifically, the mass ratio of the aluminum electrolysis waste cathode carbon block to the low melting point inorganic salt can be, for example but not limited to, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, 1:2.1, 1:2.2, 1:2.3, 1:2.4, 1:2.5, 1:2.6, 1:2.7, 1:2.8, 1:2.9, 1:3, any one of them or the range between any two of them; the roasting temperature The temperature may be, for example, but not limited to, any one of 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, or a range between any two of them; the calcination time may be, for example, but not limited to, any one of 0.5h, 0.75h, 1.0h, 1.25h, 1.5h, 1.75h, 2.0h, or a range between any two of them.

[0047] Preferably, in step S2, the mechanical activation equipment is lined with polytetrafluoroethylene; the mechanical activation leaching time is 0.1 to 1.0 h, and the rotation speed of the mechanical activation equipment is 500 to 700 r / min; the acidic solution is one or more of hydrochloric acid, sulfuric acid, nitric acid, and perchloric acid; the concentration of the acidic solution is 0.5 to 12 mol / L, and the liquid-to-solid ratio of the acidic solution to the roasting material is 5 to 20 mL / g; the fixed carbon content of the graphite is ≥99.0%, and the water washing liquid is circulated for water washing treatment. Specifically, the mechanical activation leaching time can be, for example, but not limited to, any one of 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.0h or a range between any two of them; the speed of the mechanical activation equipment can be, for example, but not limited to, any one of 500r / min, 550r / min, 600r / min, 650r / min, 700r / min or a range between any two of them; the concentration of the acidic solution can be, for example, but not limited to, 0.5mol / L, 0.1mol / L, 2mol / L, 3mol / L, 4mol / L L, 5mol / L, 6mol / L, 7mol / L, 8mol / L, 9mol / L, 10mol / L, 11mol / L, 12mol / L or any range between two of them; the liquid-to-solid ratio of the acidic solution to the roasting material can be, for example, but not limited to, 5mL / g, 6mL / g, 7mL / g, 8mL / g, 9mL / g, 10mL / g, 11mL / g, 12mL / g, 13mL / g, 14mL / g, 15mL / g, 16mL / g, 17mL / g, 18mL / g, 19mL / g, 20mL / g or any range between two of them;

[0048] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis described in the present invention, wherein: in step S3, before adding crystal seeds, the flue gas produced in step S1 is passed into the acidic leaching solution produced in step S2 to adjust the pH value to 3-6; the crystal seeds are one or more of ammonium fluoride, ammonium bifluoride, and sodium bifluoride. Specifically, the pH value can be, for example, but not limited to, any one of 3, 3.5, 4, 4.5, 5, 5.5, 6, or a range between any two of them.

[0049] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0050] Example 1

[0051] This embodiment provides a method for recovering graphite from spent cathode carbon blocks in aluminum electrolysis, comprising the following steps:

[0052] S0. Preprocessing

[0053] The aluminum electrolysis waste cathode carbon blocks are refined, screened and dried to obtain aluminum electrolysis waste cathode carbon blocks with a particle size of ≤0.15 mm;

[0054] S1. Molten salt roasting

[0055] Mechanically mixing the aluminum electrolysis waste cathode carbon block and ammonium fluoride in a mass ratio of 1:2 to obtain a mixed material; loading the mixed material into a graphite crucible and placing it in a heating device, and then calcining the mixed material with molten salt in an air atmosphere at a calcination temperature of 250° C. and a calcination time of 1.0 h to obtain a calcined material and flue gas;

[0056] S2. Mechanical Activation

[0057] The calcined material and the hydrochloric acid solution are placed in a mechanical activation device lined with polytetrafluoroethylene for leaching, the mechanical activation leaching time is 0.5h, the rotation speed of the mechanical activation device is 600r / min, the concentration of the hydrochloric acid solution is 8mol / L, the liquid-solid ratio of the hydrochloric acid solution to the calcined material is 20mL / g, and after the reaction is completed, solid-liquid separation is performed to obtain an acidic leaching solution and residual solid materials, and then the residual solid materials are washed and dried in sequence to obtain graphite and a washing liquid, and the washing liquid is recycled for washing treatment, and the fixed carbon content of the recovered graphite is 99.54wt%, the leaching rate of fluoride is 99.25%, and the decomposition rate of cyanide is 99.87%;

[0058] S3. Recycling of by-products

[0059] The flue gas generated in step S1 is introduced into the acidic leaching solution generated in step S2, and the pH value is adjusted to 4.5. Ammonium fluoride seed addition, vacuum concentration, cooling crystallization, solid-liquid separation, and freeze drying are sequentially performed to obtain low-melting-point inorganic salts and supernatant, which are respectively returned to the molten salt roasting link and the mechanical activation link for water washing processes for recycling. The recovery rate of the low-melting-point inorganic salt is 91.2%.

[0060] Example 2

[0061] This embodiment provides a method for recovering graphite from spent cathode carbon blocks in aluminum electrolysis, comprising the following steps:

[0062] S0. Preprocessing

[0063] The aluminum electrolysis waste cathode carbon blocks are refined, screened and dried to obtain aluminum electrolysis waste cathode carbon blocks with a particle size of ≤5mm;

[0064] S1. Molten salt roasting

[0065] Mechanically mixing the aluminum electrolysis waste cathode carbon block and ammonium fluoride in a mass ratio of 1:3 to obtain a mixed material; loading the mixed material into a graphite crucible and placing it in a heating device, and then calcining the mixed material with molten salt in an air atmosphere at a calcination temperature of 250° C. and a calcination time of 2.0 h to obtain a calcined material and flue gas;

[0066] S2. Mechanical Activation

[0067] The calcined material and the hydrochloric acid solution are placed in a mechanical activation device lined with polytetrafluoroethylene for leaching, the mechanical activation leaching time is 1.0h, the rotation speed of the mechanical activation device is 700r / min, the concentration of the hydrochloric acid solution is 10mol / L, the liquid-solid ratio of the hydrochloric acid solution to the calcined material is 20mL / g, and after the reaction is completed, solid-liquid separation is performed to obtain an acidic leaching solution and residual solid materials, and then the residual solid materials are washed and dried in sequence to obtain graphite and a washing liquid, and the washing liquid is recycled for washing treatment, and the fixed carbon content of the recovered graphite is 99.12wt%, the leaching rate of fluoride is 99.05%, and the decomposition rate of cyanide is 99.57%;

[0068] S3. Recycling of by-products

[0069] The flue gas generated in step S1 is introduced into the acidic leaching solution generated in step S2, and the pH value is adjusted to 5.5. Ammonium fluoride seed addition, vacuum concentration, cooling crystallization, solid-liquid separation, and freeze drying are sequentially performed to obtain low-melting-point inorganic salts and supernatant, which are respectively returned to the molten salt roasting link and the mechanical activation link for water washing processes for recycling. The recovery rate of the low-melting-point inorganic salt is 89.8%.

[0070] Example 3

[0071] This embodiment provides a method for recovering graphite from spent cathode carbon blocks in aluminum electrolysis, comprising the following steps:

[0072] S0. Preprocessing

[0073] The aluminum electrolysis waste cathode carbon blocks are refined, screened and dried to obtain aluminum electrolysis waste cathode carbon blocks with a particle size of ≤0.15 mm;

[0074] S1. Molten salt roasting

[0075] Mechanically mixing the aluminum electrolysis waste cathode carbon block and ammonium fluoride in a mass ratio of 1:2.5 to obtain a mixed material; loading the mixed material into a graphite crucible and placing it in a heating device, and then calcining it with molten salt in an air atmosphere at a calcination temperature of 200° C. for a calcination time of 2.0 h to obtain a calcined material and flue gas;

[0076] S2. Mechanical Activation

[0077] The calcined material and the sulfuric acid solution are placed in a mechanical activation device lined with polytetrafluoroethylene for leaching, the mechanical activation leaching time is 1.0h, the rotation speed of the mechanical activation device is 650r / min, the concentration of the sulfuric acid solution is 4mol / L, the liquid-solid ratio of the sulfuric acid solution and the calcined material is 18mL / g, and after the reaction is completed, solid-liquid separation is performed to obtain an acidic leaching solution and residual solid materials, and then the residual solid materials are washed and dried in sequence to obtain graphite and a washing liquid, and the washing liquid is recycled for washing treatment, and the fixed carbon content of the recovered graphite is 99.72wt%, the leaching rate of fluoride is 99.46%, and the decomposition rate of cyanide is 99.91%;

[0078] S3. Recycling of by-products

[0079] The flue gas generated in step S1 is introduced into the acidic leaching solution generated in step S2, and the pH value is adjusted to 5. Ammonium fluoride seed addition, vacuum concentration, cooling crystallization, solid-liquid separation, and freeze drying are performed in sequence to obtain low-melting-point inorganic salts and supernatant, which are returned to the washing process of the molten salt roasting link and the mechanical activation link for recycling. The recovery rate of the low-melting-point inorganic salt is 92.3%.

[0080] Example 4

[0081] This embodiment provides a method for recovering graphite from spent cathode carbon blocks in aluminum electrolysis, comprising the following steps:

[0082] S0. Preprocessing

[0083] The aluminum electrolysis waste cathode carbon blocks are refined, screened and dried to obtain aluminum electrolysis waste cathode carbon blocks with a particle size of ≤1 mm;

[0084] S1. Molten salt roasting

[0085] Mechanically mixing the aluminum electrolysis waste cathode carbon block and ammonium bifluoride in a mass ratio of 1:3 to obtain a mixed material; loading the mixed material into a graphite crucible and placing it in a heating device, and then calcining the mixed material with molten salt in an air atmosphere at a calcination temperature of 250° C. and a calcination time of 1.5 hours to obtain a calcined material and flue gas;

[0086] S2. Mechanical Activation

[0087] The calcined material and the hydrochloric acid solution are placed in a mechanical activation device lined with polytetrafluoroethylene for leaching, the mechanical activation leaching time is 1.0h, the rotation speed of the mechanical activation device is 500r / min, the concentration of the hydrochloric acid solution is 8mol / L, the liquid-solid ratio of the hydrochloric acid solution to the calcined material is 20mL / g, and after the reaction is completed, solid-liquid separation is performed to obtain an acidic leaching solution and residual solid materials, and then the residual solid materials are washed and dried in sequence to obtain graphite and a washing liquid, and the washing liquid is recycled for washing treatment, and the fixed carbon content of the recovered graphite is 99.21wt%, the leaching rate of fluoride is 99.13%, and the decomposition rate of cyanide is 99.62%;

[0088] S3. Recycling of by-products

[0089] The flue gas generated in step S1 is introduced into the acidic leaching solution generated in step S2, the pH value is adjusted to 5, and ammonium bifluoride seed addition, vacuum concentration, cooling crystallization, solid-liquid separation, and freeze drying are performed in sequence to obtain low-melting-point inorganic salts and supernatant, which are returned to the washing process of the molten salt roasting link and the mechanical activation link for recycling, and the recovery rate of the low-melting-point inorganic salt is 85.9%.

[0090] The present invention adopts low melting point inorganic salt to carry out molten salt roasting treatment on waste cathode carbon blocks from aluminum electrolysis to obtain roasted materials and flue gas, places the roasted materials and acidic solution in mechanical activation equipment for leaching, carries out solid-liquid separation after the reaction is completed to obtain acidic leaching solution and residual solid materials, then washes and dries the residual solid materials in sequence to obtain graphite and washing solution; at the same time, a recycling process for by-products such as flue gas and acidic leaching solution is designed to avoid environmental pollution of waste gas and waste liquid, realize green recovery of high-quality graphite resources of waste cathode carbon blocks from aluminum electrolysis, safe dissociation of cyanide / fluorine toxic components and regeneration and recycling of molten salt roasting agents, and has the characteristics of high efficiency, environmental protection and simple process.

[0091] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis, characterized in that: The steps include: S1. Molten salt roasting Mechanically mixing the aluminum electrolysis waste cathode carbon block and the low melting point inorganic salt in a mass ratio of 1:1-3 to obtain a mixed material; the low melting point inorganic salt is one or more of ammonium fluoride, ammonium bifluoride, and sodium bifluoride; loading the mixed material into a graphite crucible and placing it in a heating device, and then calcining the molten salt in an air atmosphere at a calcination temperature of 100-250° C. and a calcination time of 0.5-2.0 h to obtain a calcined material and flue gas; S2. Mechanical Activation The calcined material and the acidic solution are placed in a mechanical activation device for leaching, the concentration of the acidic solution is 0.5-12 mol / L, and the liquid-solid ratio of the acidic solution to the calcined material is 5-20 mL / g; the mechanical activation leaching time is 0.1-1.0 h, and the speed of the mechanical activation device is 500-700 r / min; after the reaction is completed, solid-liquid separation is performed to obtain an acidic leaching solution and residual solid materials, and then the residual solid materials are washed and dried in turn to obtain graphite and a washing solution, wherein the fixed carbon content of the graphite is ≥99.0%; S3. Recycling of by-products The flue gas generated in step S1 is introduced into the acidic leaching solution generated in step S2, and seed addition, vacuum concentration, cooling crystallization, solid-liquid separation, and freeze drying are performed in sequence to obtain low-melting-point inorganic salts and supernatant, which are returned to the molten salt roasting step and the mechanical activation step for water washing processes for recycling.

2. The method according to claim 1, characterized in that Before step S1, the following steps are also included: S0. Preprocessing The aluminum electrolysis waste cathode carbon blocks are refined, screened and dried to obtain aluminum electrolysis waste cathode carbon blocks with a particle size of ≤5mm.

3. The method according to any one of claims 1 to 2, characterized in that: In step S2, the acidic solution is one or more of hydrochloric acid, sulfuric acid, nitric acid, and perchloric acid.

4. The method according to any one of claims 1 to 2, characterized in that: In step S2, the washing liquid is circulated for washing treatment.

5. The method according to claim 1, characterized in that In step S3, before adding the seed crystals, the flue gas produced in step S1 is introduced into the acidic leaching solution produced in step S2 to adjust the pH value to 3-6.

6. The method according to claim 1, characterized in that In step S3, the seed crystal is one or more of ammonium fluoride, ammonium bifluoride, and sodium bifluoride.

Citation Information

Patent Citations

  • Method for recovering graphite from waste cathode carbon blocks in electrolytic aluminium production

    CN101811695A

  • Sodium-embedded graphite prepared from aluminum electrolysis waste cathode and application thereof

    CN110180862A

  • Method for recovering carbon and electrolyte from aluminum electrolysis waste cathode carbon blocks

    CN110408959A

  • Method for removing trace beryllium elements from waste cathodes of aluminum electrolysis

    CN112340722A

  • Production of molded active carbon

    JP2000247622A

Cited By

  • Method for preparing prebaked anode by blending recycled graphite of aluminum electrolysis waste cathode carbon block

    CN116288533A

  • A method for preparing prebaked anodes by blending graphite recovered from aluminum electrolysis spent cathode blocks

    CN116288533B