Adult diaper core structure with excellent antibacterial and anti-odor properties and its preparation process

By using crosslinks of γ-polyglutamic acid, ε-polylysine, and β-1,3 glucan as antibacterial and odor-resistant films, the problem of insufficient antibacterial and odor-resistant performance of adult diapers is solved, and high efficiency is achieved The antibacterial effect and liquid absorption performance have significantly improved the safety and comfort of diapers.

CN115920111BActive Publication Date: 2024-11-05HANGZHOU COCO HEALTHCARE PRODS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211265306.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-17
Publication Date
2024-11-05
Estimated Expiration
2042-10-17

AI Technical Summary

Technical Problem

The antibacterial and odor-resistant properties of existing adult diapers are poor, especially in the case of long-term use and high urine volume, which can easily lead to bacterial growth and foul odor spread. It is difficult to improve the effect without affecting the absorption performance when the antibacterial agent is added.

Method used

Using γ-polyglutamic acid, ε-polylysine, β-1,3 glucan as raw materials, water-soluble crosslinking is formed through crosslinking reaction, as an antibacterial and odor-resistant film material, and infiltrates the nonwoven coating layer. Or spray the absorbent core layer, combine ammonia water-normal saline for passivation reaction and dry it to form an antibacterial and odor-resistant film material, maintaining water absorption, water locking and breathable properties, while significantly improving the antibacterial effect.

Benefits of technology

It significantly improves the antibacterial and odor resistance of diapers, can effectively absorb urine and protect the skin, significantly improve the antibacterial effect without affecting the absorption speed and comfort. The test results show the inhibition of E. coli and Staphylococcus aureus. The bacterial rate reaches more than 98%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003892884660000081
    Figure BDA0003892884660000081
Patent Text Reader

Abstract

The present invention relates to an adult diaper core structure with excellent antibacterial and anti-odor performance and a preparation process thereof, including a non-woven fabric coating layer and a fluff pulp absorption core layer, wherein the non-woven fabric coating layer is infiltrated with an antibacterial and anti-odor film material, and / or the fluff pulp absorption core layer is sprayed with an antibacterial and anti-odor film material, wherein the antibacterial and anti-odor film material is made of γ-polyglutamic acid, ε-polylysine, and β-1,3-glucan as raw materials, and then ammonia water-physiological saline is added to the cross-linking reaction system for passivation reaction, and finally obtained by drying. The present invention forms a water-soluble crosslinked body of γ-polyglutamic acid-ε-polylysine-β-1,3-glucan capable of forming a gel film through the crosslinking of polyglutamic acid, ε-polylysine and β-1,3-glucan, and after treating the coating layer non-woven fabric, it is used for diapers, that is, it does not affect the air permeability, high dispersion and permeability of the coating layer non-woven fabric, and can inhibit bacteria and odor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an adult diaper core structure, in particular to an adult diaper core structure with excellent antibacterial and deodorizing properties and a preparation process thereof, belonging to the technical field of sanitary product materials. Background Art

[0002] Diapers are disposable products that can be discarded after use. The diapers of the prior art are composed of three main parts: a surface coating layer, an absorbent core layer and a base fabric. The surface coating layer can also be called a coating layer. The absorbent core layer can also be called an absorbent core, or an absorbent. The coating layer is close to the user's body, which can promote the rapid penetration of urine and effectively prevent back-seepage, so that the surface of the diaper remains dry. At present, the coating layer of diapers on the domestic market is basically a non-woven surface layer. The breathable non-woven fabric can improve the air permeability inside the diaper, and water vapor can flow outside the diaper, timely discharge moisture and heat, effectively reduce the chance of diaper rash, and is soft, comfortable and does not irritate the skin. The absorbent core layer can also be called an absorbent core. The main function of the absorbent core layer is to capture and quickly absorb urine, disperse urine, or diffuse it into the entire core layer through capillary action, and finally absorb and store urine. At present, the absorbent core layer of diapers on the domestic market is mainly a layered structure composed of pure wood pulp (fluff pulp) and super absorbent resin (SAP). The base fabric is the outermost layer of the diaper, which is impermeable and can prevent moisture from seeping out of the absorbent core layer. The base fabrics of many diapers abroad have been made of non-woven fabrics, which feel more comfortable, but due to the high price, the base fabrics of diapers in the domestic market are still mainly made of PE film.

[0003] Adult diapers have a large amount of urine and are used for a long time, so the diaper finishing and absorption capacity are relatively high. In view of the fact that the price of polymers is much more expensive than that of fluff pulp, the absorbent core of adult diapers is mainly made of fluff pulp. In addition, due to the long use time of adult diapers and the patient's own factors (taking medicines, ward environment, etc.), bacterial growth and odor emission during use are inevitable. Therefore, it is very necessary to add antibacterial agents to the diaper core. How to add antibacterial agents to improve the antibacterial effect without affecting the absorption performance requires comprehensive consideration. The present invention aims to solve this technical problem. Summary of the invention

[0004] One of the purposes of the present invention is to solve the shortcomings of the prior art adult diapers that have poor antibacterial and anti-odor properties, and to provide an adult diaper core structure with excellent antibacterial and anti-odor properties and a preparation process thereof.

[0005] The technical solution adopted by the present invention to solve the technical problem is:

[0006] The core structure of adult diapers includes a non-woven fabric covering layer and a fluff pulp absorption core layer, characterized in that: the non-woven fabric covering layer is infiltrated with an antibacterial and anti-odor film material, and / or the fluff pulp absorption core layer is sprayed with an antibacterial and anti-odor film material, the antibacterial and anti-odor film material is made of γ-polyglutamic acid, ε-polylysine, and β-1,3 glucan as raw materials, and is cross-linked by a cross-linking agent, and then ammonia water-normal saline is added to the cross-linking reaction system for passivation reaction, and finally dried to obtain it.

[0007] There are very active -COOH groups in the molecular chain of polyglutamic acid (γ-PGA), which are found to have many available functions, such as water absorption, moisturizing and adsorption of heavy metals. At the same time, monomeric glutamic acid belongs to amino acids, which will not cause any pollution after degradation and is an environmentally friendly material. γ-polyglutamic acid has strong water retention and sustained release because it contains more carboxyl groups and active groups. In addition, γ-PGA is a multi-functional ingredient that combines moisturizing, whitening, antibacterial and skin health. While quickly achieving deep penetration and hydration, it comprehensively inhibits melanin production, fades spots, continuously decomposes aging keratin, and keeps the skin fresh and tender. ε-polylysine has good bactericidal ability and thermal stability, and is a biological preservative with excellent antiseptic properties and huge commercial potential. The use of ε-polylysine and other natural antibacterial agents in combination has obvious synergistic effects and can improve its antibacterial ability. The present invention forms a water-soluble crosslinked body of γ-polyglutamic acid-ε-polylysine-β-1,3 glucan capable of forming a gel film by crosslinking polyglutamic acid, ε-polylysine and β-1,3 glucan. After the coating layer non-woven fabric is treated, the crosslinked body is used for diapers, which does not affect the air permeability, high dispersion and permeability of the coating layer non-woven fabric, and can inhibit bacteria and odor.

[0008] The present invention protects three schemes, one of which is a coating layer non-woven fabric loaded membrane material. In this case, if there is back-seepage urine, the γ-polyglutamic acid-ε-polylysine-β-1,3-glucan water-soluble cross-linked membrane layer has good water absorption and water locking properties and can absorb the back-seepage urine. At the same time, the dissolved part of the γ-polyglutamic acid-ε-polylysine-β-1,3-glucan water-soluble cross-linked body can form a protective film even if it adheres to the skin, thereby protecting the skin and inhibiting bacteria and odor.

[0009] In the second option, the core layer of fluff pulp is loaded with antibacterial and anti-odor film material. The specific surface area of ​​the fluff pulp forms a uniformly distributed, three-dimensional, multi-site antibacterial and anti-odor zone, which can significantly improve the antibacterial and anti-odor effect.

[0010] In the third option, both the covering layer non-woven fabric and the core layer fluff pulp are loaded with antibacterial and anti-odor film materials, which can not only absorb and lock moisture, but also inhibit odor and bacteria, and can effectively protect the user's skin.

[0011] Preferably, the mass ratio of γ-polyglutamic acid, ε-polylysine and β-1,3 glucan is (1-3): (1-2): (0.5-1).

[0012] Preferably, the mass ratio of γ-polyglutamic acid, ε-polylysine and β-1,3 glucan is 2:1:1.

[0013] Preferably, the crosslinking agent is any one of polycarbodiimide crosslinking agent, trimethylolpropane trimethacrylate crosslinking agent, glutaraldehyde crosslinking agent, and succinaldehyde crosslinking agent, and the mass dosage of the crosslinking agent is 1-5% of the mass of the raw material.

[0014] Preferably, the crosslinking agent is a polycarbodiimide crosslinking agent and / or a trimethylolpropane trimethacrylate crosslinking agent.

[0015] Preferably, the ammonia concentration of the ammonia water-physiological saline solution is 2-4%, the volume ratio of the ammonia water to the cross-linking reaction system is 1:(2-3), and the passivation reaction time is 1-2 hours.

[0016] Preferably, the volume of the physiological saline is 2-3 times the volume of the system after the passivation reaction, and the purification times are 2-3 times.

[0017] An adult diaper core structure, the film material is prepared as follows:

[0018] Step S1: weighing the formulated amount of γ-polyglutamic acid, ε-polylysine, and β-1,3 glucan, dissolving them in 2-3 times of normal saline, filtering to remove impurities to obtain a raw material solution, and heating the raw material solution to 40-45° C. for standby use;

[0019] Step S2: Take a cross-linking agent and add it dropwise to the raw material solution of step S2, stirring while adding, and react for 1-2 hours;

[0020] Step S3: Take ammonia water-physiological saline and add it dropwise to the cross-linking reaction system of step S2, stirring while adding, and react for 0.5-1h;

[0021] Step S4: The reaction liquid of step S3 is dried to obtain a membrane material, wherein the drying is carried out by spray drying, and the inlet air temperature of the spray drying is 190-210°C, and the outlet air temperature is 150-160°C.

[0022] Preferably, the method for loading the antibacterial and anti-odor film material on the non-woven fabric is: the film material is prepared into a 10-15% solution with deionized water, 0.5-1% polyvinyl pyrrolidone by weight of the film material is added, and then the non-woven fabric is soaked for 3-5 minutes, and the soaked non-woven fabric is dried; the method for spraying the antibacterial and anti-odor film material on the fluff pulp absorption core layer is: the film material is prepared into a 10-15% solution with deionized water, 0.5-1% polyvinyl pyrrolidone by weight of the film material is added, and then the solution is evenly sprayed into the fluff pulp at a volume ratio of 1:5, and then it is dried.

[0023] The beneficial effect of the present invention is that the present invention protects three schemes, one of which is a coating layer non-woven fabric loaded membrane material. In this case, if there is back-seepage urine, since the γ-polyglutamic acid-ε-polylysine-β-1,3-glucan water-soluble cross-linked membrane layer has good water absorption and water locking properties, it can absorb the back-seepage urine. At the same time, the dissolved part of the γ-polyglutamic acid-ε-polylysine-β-1,3-glucan water-soluble cross-linked body can form a protective film even if it adheres to the skin, thereby protecting the skin and inhibiting bacteria and odor.

[0024] In the second option, the core layer of fluff pulp is loaded with antibacterial and anti-odor film material. The specific surface area of ​​the fluff pulp forms a uniformly distributed, three-dimensional, multi-site antibacterial and anti-odor zone, which can significantly improve the antibacterial and anti-odor effect.

[0025] In the third option, both the covering layer non-woven fabric and the core layer fluff pulp are loaded with antibacterial and anti-odor film materials, which can not only absorb and lock moisture, but also inhibit odor and bacteria, and can effectively protect the user's skin. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further described in detail below through specific embodiments.

[0027] Embodiment 1:

[0028] The core structure of adult diapers includes a non-woven fabric covering layer and a fluff pulp absorption core layer, wherein the non-woven fabric covering layer is impregnated with an antibacterial and anti-odor film material, wherein the antibacterial and anti-odor film material is made of γ-polyglutamic acid, ε-polylysine, and β-1,3-glucan as raw materials, and is cross-linked by a cross-linking agent, and then ammonia water-physiological saline is added to the cross-linking reaction system for passivation reaction, and finally dried;

[0029] The mass ratio of the gamma-polyglutamic acid, epsilon-polylysine and beta-1,3 glucan is 1:1:0.5.

[0030] The cross-linking agent is a polycarbodiimide cross-linking agent, and the mass dosage of the cross-linking agent is 1% of the mass of the raw material.

[0031] The ammonia concentration of the ammonia water-physiological saline solution is 2%, the volume ratio of the ammonia water to the cross-linking reaction system is 1:2, and the passivation reaction time is 1 hour.

[0032] The volume of the physiological saline was twice the volume of the system after the passivation reaction, and the purification times were 3 times.

[0033] The preparation method of the membrane material is as follows:

[0034] Step S1: weighing the formulated amount of γ-polyglutamic acid, ε-polylysine, and β-1,3-glucan, dissolving them in 2 times of normal saline, filtering to remove impurities to obtain a raw material solution, and heating the raw material solution to 40° C. for standby use;

[0035] Step S2: Take a cross-linking agent and add it dropwise to the raw material solution of step S2, stirring while adding, and react for 1 hour;

[0036] Step S3: Take ammonia water-physiological saline and add it dropwise to the cross-linking reaction system of step S2, stirring while adding, and react for 0.5h;

[0037] Step S4: The reaction liquid of step S3 is dried to obtain a membrane material. The drying is carried out by spray drying. The inlet air temperature of the spray drying is 190°C and the outlet air temperature is 150°C.

[0038] The method of loading the antibacterial and anti-odor film material on the non-woven fabric is as follows: the film material is prepared into a 10% solution with deionized water, 0.5% polyvinyl pyrrolidone by weight of the film material is added, and then the non-woven fabric is soaked for 3 minutes, and the soaked non-woven fabric is dried.

[0039] Embodiment 2:

[0040] The core structure of adult diapers includes a non-woven fabric covering layer and a fluff pulp absorption core layer. The fluff pulp absorption core layer is spray-loaded with an antibacterial and anti-odor film material. The antibacterial and anti-odor film material is made of γ-polyglutamic acid, ε-polylysine, and β-1,3-glucan as raw materials, and is cross-linked by a cross-linking agent, and then ammonia water-physiological saline is added to the cross-linking reaction system for a passivation reaction, and finally dried. The mass ratio of γ-polyglutamic acid, ε-polylysine and β-1,3-glucan is 3:2:1.

[0041] The crosslinking agent is trimethylolpropane trimethacrylate crosslinking agent, and the mass dosage of the crosslinking agent is 5% of the mass of the raw material.

[0042] The ammonia concentration of the ammonia water-physiological saline solution is 4%, the volume ratio of the ammonia water to the cross-linking reaction system is 1:3, and the passivation reaction time is 2 hours.

[0043] The volume of the physiological saline is 3 times the volume of the system after the passivation reaction, and the purification times are 3 times.

[0044] The preparation method of the membrane material is as follows:

[0045] Step S1: weighing the formulated amount of γ-polyglutamic acid, ε-polylysine, and β-1,3-glucan, dissolving them in 3 times of normal saline, filtering to remove impurities to obtain a raw material solution, and heating the raw material solution to 45° C. for standby use;

[0046] Step S2: Take a cross-linking agent and add it dropwise to the raw material solution of step S2, stirring while adding, and react for 2 hours;

[0047] Step S3: Take ammonia water-physiological saline and add it dropwise to the cross-linking reaction system of step S2, stirring while adding, and react for 1 hour;

[0048] Step S4: The reaction liquid of step S3 is dried to obtain a membrane material. The drying is carried out by spray drying. The inlet air temperature of the spray drying is 210°C and the outlet air temperature is 160°C.

[0049] The method of spraying the antibacterial and odor-resistant film material on the fluff pulp absorption core layer is as follows: the film material is prepared into a 15% solution with deionized water, 1% polyvinyl pyrrolidone by weight of the film material is added, and then the solution and the fluff pulp are evenly sprayed into the fluff pulp at a volume ratio of 1:5, and then dried.

[0050] Embodiment 3:

[0051] The core structure of adult diapers includes a non-woven fabric covering layer and a fluff pulp absorption core layer. The non-woven fabric covering layer is impregnated with an antibacterial and anti-odor film material, and the fluff pulp absorption core layer is sprayed with an antibacterial and anti-odor film material. The antibacterial and anti-odor film material is made of γ-polyglutamic acid, ε-polylysine, and β-1,3-glucan as raw materials, and is cross-linked by a cross-linking agent, and then ammonia water-normal saline is added to the cross-linking reaction system for a passivation reaction, and finally dried to obtain the obtained film material.

[0052] The mass ratio of the gamma-polyglutamic acid, epsilon-polylysine and beta-1,3 glucan is 2:1:1.

[0053] The cross-linking agent is a polycarbodiimide cross-linking agent, and the mass dosage of the cross-linking agent is 3% of the mass of the raw material.

[0054] The ammonia concentration of the ammonia water-physiological saline solution is 3%, the volume ratio of the ammonia water to the cross-linking reaction system is 1:2.5, and the passivation reaction time is 1.5 hours.

[0055] The volume of the physiological saline was 2.5 times the volume of the system after the passivation reaction, and the purification times were 3 times.

[0056] The preparation method of the membrane material is as follows:

[0057] Step S1: weighing the formulated amount of γ-polyglutamic acid, ε-polylysine, and β-1,3-glucan, dissolving them in 2 times of normal saline, filtering to remove impurities to obtain a raw material solution, and heating the raw material solution to 40° C. for standby use;

[0058] Step S2: Take a cross-linking agent and add it dropwise to the raw material solution of step S2, stirring while adding, and react for 1 hour;

[0059] Step S3: Take ammonia water-physiological saline and add it dropwise to the cross-linking reaction system of step S2, stirring while adding, and react for 1 hour;

[0060] Step S4: The reaction liquid of step S3 is dried to obtain a membrane material, wherein the drying is carried out by spray drying, and the inlet air temperature of the spray drying is 190°C and the outlet air temperature is 160°C.

[0061] The method of loading the antibacterial and anti-odor film material on the non-woven fabric is as follows: the film material is prepared into a 10% solution with deionized water, 0.5% polyvinyl pyrrolidone by weight of the film material is added, and then the non-woven fabric is soaked for 5 minutes, and the soaked non-woven fabric is dried; the method of spraying the antibacterial and anti-odor film material on the fluff pulp absorption core layer is as follows: the film material is prepared into a 10% solution with deionized water, 1% polyvinyl pyrrolidone by weight of the film material is added, and then the solution is evenly sprayed into the fluff pulp at a volume ratio of 1:5, and then it is dried.

[0062] Example 1-3 Adult diapers processed with nonwoven fabric as the covering layer or core layer are used for moisture absorption and comfort performance testing. The specific operation is as follows:

[0063] 1. Test method:

[0064] 1.1 Absorption speed:

[0065] (A) Test equipment and reagents

[0066] (1) Balance: accuracy 0.01g, 1 unit

[0067] (2) Standard pouring cylinder: about 545g, diameter 2.5cm

[0068] (3) Graduated cylinder

[0069] (4) Several sheets of medium-speed chemical qualitative analysis filter paper (GB / T 1914)

[0070] (5) Standard briquetting, Weight is (1.2±0.002)kg (can generate 1.5kPa pressure)

[0071] (6) Stopwatch: accuracy 0.01S, 1 piece

[0072] (7) Test solution: 0.9% saline solution with food coloring added (the sample was processed and tested under standard atmospheric conditions, i.e., (23 ± 1) °C, (50 ± 2)% rh)

[0073] (8)Steel ruler

[0074] (2) Operation process

[0075] (1) Lay the core to be tested flat, draw a line at the center of the core as the liquid adding point, and the sample length is 400 mm.

[0076] (B) Use a measuring cylinder to measure a certain amount of test solution (as shown below), pour it into the liquid guide tube, let the liquid flow to the surface of the sample, and start timing. When the liquid on the surface of the guide layer disappears, the timing ends. The time at this time is recorded as t1, which is the absorption rate.

[0077] Liquid volume: S / M / L / XL (100ml per time).

[0078] 1.2 Saturation absorption:

[0079] (A) Test solutions and instruments

[0080] (1) Test solution: 0.9% saline

[0081] (2) Balance (accurate to 0.1)

[0082] (3) Stopwatch

[0083] (4) 200 mesh nylon bag

[0084] (B) Operation process

[0085] (1) Measure the wet weight A of the nylon bag and the weight B after drying in advance.

[0086] (2) Cut a 0.5 m long piece of the core to be tested and weigh it, record it as C.

[0087] (3) The core to be tested is placed in a nylon bag and completely immersed in saline for 30 minutes.

[0088] (4) After soaking, hang it on a drain rack for 10 minutes.

[0089] (5) After 10 minutes, weigh the entire weight of the core to be tested and the nylon bag, and record it as D. The saturated absorption capacity of the core to be tested = DAC.

[0090] 1.2 Comfort: 200 long-term bedridden elderly patients aged 50-60 were selected to evaluate the redness and swelling of the skin after using diapers.

[0091] 2. Test results:

[0092]

[0093] From the above test data, it can be seen that the non-woven diaper of the present invention does not affect the liquid absorption speed. In addition, the comfort and safety are also significantly improved, and it is observed that the samples to be tested do not clump. The antibacterial experiment shows that the antibacterial rates of Examples 1-3 against Escherichia coli are 98.2%, 98.1%, and 99.2%, respectively, and the antibacterial rates of Examples 1-3 against Staphylococcus aureus are 94.2%, 94.8%, and 95.5%, respectively.

[0094] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.

Claims

1. The core structure of adult diapers with excellent antibacterial and anti-odor properties includes a non-woven fabric covering layer and a fluff pulp absorption core layer. Features: The non-woven fabric covering layer is impregnated with an antibacterial and anti-odor film material, and the fluff pulp absorption core layer is sprayed with an antibacterial and anti-odor film material. The antibacterial and anti-odor film material is made of γ-polyglutamic acid, ε-polylysine, and β-1,3 glucan as raw materials, and is cross-linked by a cross-linking agent, and then ammonia water-physiological saline is added to the cross-linking reaction system for passivation reaction, and finally dried to obtain the film. The mass ratio of γ-polyglutamic acid, ε-polylysine and β-1,3 glucan is (1-3): (1-2): (0.5-1); The crosslinking agent is any one of polycarbodiimide crosslinking agent, trimethylolpropane trimethacrylate crosslinking agent, glutaraldehyde crosslinking agent, and succinaldehyde crosslinking agent, and the mass dosage of the crosslinking agent is 1-5% of the mass of the raw material; The preparation method of the membrane material is as follows: Step S1: weighing the formulated amount of γ-polyglutamic acid, ε-polylysine, and β-1,3 glucan, dissolving them in 2-3 times of normal saline, filtering to remove impurities to obtain a raw material solution, and heating the raw material solution to 40-45° C. for standby use; Step S2: Take a cross-linking agent and add it dropwise to the raw material solution of step S1, stirring while adding, and react for 1-2 hours; Step S3: Take ammonia water-physiological saline and add it dropwise to the cross-linking reaction system of step S2, stirring while adding, and react for 0.5-1h; Step S4: The reaction liquid of step S3 is dried to obtain a film material, wherein the drying is carried out by spray drying, and the inlet air temperature of the spray drying is 190-210°C and the outlet air temperature is 150-160°C; The method of loading the antibacterial and anti-odor film material on the non-woven fabric is as follows: the film material is prepared into a 10-15% solution with deionized water, 0.5-1% polyvinyl pyrrolidone by weight of the film material is added, and then the non-woven fabric is soaked for 3-5 minutes, and the soaked non-woven fabric is dried; the method of spraying the antibacterial and anti-odor film material on the fluff pulp absorption core layer is as follows: the film material is prepared into a 10-15% solution with deionized water, 0.5-1% polyvinyl pyrrolidone by weight of the film material is added, and then the solution is evenly sprayed into the fluff pulp at a volume ratio of 1:5, and then it is dried.

2. The core structure of adult diapers with excellent antibacterial and anti-odor properties according to claim 1, Features: The mass ratio of the gamma-polyglutamic acid, epsilon-polylysine and beta-1,3 glucan is 2:1:

1.

3. The core structure of adult diapers with excellent antibacterial and anti-odor properties according to claim 1, Features: The crosslinking agent is a polycarbodiimide crosslinking agent and / or a trimethylolpropane trimethacrylate crosslinking agent.

4. The core structure of adult diapers with excellent antibacterial and anti-odor properties according to claim 1, Features: The ammonia concentration of the ammonia water-physiological saline solution is 2-4%, the volume ratio of the ammonia water to the cross-linking reaction system is 1:(2-3), and the passivation reaction time is 1-2 hours.