A printing method for SLM high-density diamond metal-based composite material
Through SLM technology and heavy liquid separation technology, the problem of low density of 3D printed diamond/metal matrix composites is solved, the advantages of high density and complex structure forming are achieved, and the thermal conductivity and overall quality of the print parts are improved.
Patent Information
- Application Number
- CN202211666768.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The density of existing 3D printed diamond/metal matrix composites is low, resulting in insufficient thermal conductivity and difficult deformation during full densification, which affects the quality of the print.
Using SLM technology, by establishing a CAD model and layering the diamond/metal matrix composite material, the secondary densification of the metal layer forms a skeleton, and then laser printing is performed to gradually increase the density of the print, combining heavy liquid separation and post-processing Technology to achieve high density print parts production.
The high density of the print parts (density reaches 93% to 96%) is achieved, the volume changes before and after full densification are reduced, and the forming ability and thermal conductivity of complex structural parts are improved.
Smart Images

Figure CN115921895B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for 3D printing a diamond / metal matrix composite material. Background Art
[0002] With the iteration and update of electronic devices, heat dissipation has gradually become an important reason limiting the performance improvement of components. Thermal management materials are one of the important ways to dissipate heat for electronic components. Diamond / metal matrix composites have attracted widespread attention due to their excellent thermal conductivity and low thermal expansion coefficient, and are known as the next generation of thermal management materials. With the popularization of 5G, the Internet of Things, and smart phones, the application scenarios of electronic components have become complex and diverse, and the shapes of thermal management devices have also become complex and diverse. 3D printing has attracted widespread attention due to its advantages in the forming of complex structural parts, and it has provided a way for the near-net forming of diamond / metal matrix composites that are difficult to perform post-processing processes such as cutting and polishing.
[0003] At present, powder bed additive manufacturing methods such as laser selective melting (SLM), electron beam selective sintering (EBM), and binder jetting (BJ) are the main means of 3D printing of diamond / metal matrix composites. However, due to the poor wettability of diamond and metal, the effect of diamond / metal matrix composites is limited, and there are a large number of pores inside the printed parts, which is manifested as low density of the printed parts in the macroscopic way. Usually, researchers start from the printing raw materials and coat the diamond powder with transition layer metals such as Ti, Cr, Mo, and W to reduce the thermal resistance caused by the pores between the interfaces, increase the density of the printed parts, and improve the thermal conductivity of the diamond / metal matrix composite printed parts. However, since it is difficult for the metal coating to fill the pores between the powder bed particles, it is often necessary to fully densify the printed parts under high temperature and high pressure (after densification, the density is >99%). The process of full densification inevitably leads to changes in the volume of the printed part. Especially for particles with extremely high hardness such as diamond, the overall densification process will not produce deformation, and the overall deformation can only be coordinated by metal deformation, which undoubtedly increases the difficulty of densification of the printed part during post-processing. Therefore, before the full densification process, obtaining a high-density print can not only reduce the change in the volume of the print before and after full densification, but also is a necessary prerequisite for improving the full densification effect of diamond / metal matrix composite materials (higher density, smaller irregular deformation). Summary of the invention
[0004] The present invention aims to solve the technical problem of low density of current 3D printed diamond / metal matrix composite materials, and provide a SLM printing method for high-density diamond metal matrix composite materials.
[0005] The printing method of the SLM high-density diamond metal-based composite material of the present invention is carried out according to the following steps:
[0006] 1. Establish a CAD model of the printed part, slice the CAD model, and obtain a slice A with a required layer thickness of h0; set the thickness of the metal layer powder material layer to h1, and the thickness of the diamond / metal matrix composite material layer to h2, and h0=h1+h2;
[0007] 2. ①. Fill the lifting platform in the printing cylinder with metal powder, and the lifting platform in the powder feeding cylinder is empty and the lifting platform is at the highest point in the powder feeding cylinder (such as Figure 2 The state of the upper left corner area); raise the lifting platform in the printing cylinder to a height of h1, and lower the lifting platform in the powder feeding cylinder to a height of h1 (such as Figure 2 The round roller of the printer moves from the printing cylinder to the powder feeding cylinder to feed the metal powder with a height of h1 in the original printing cylinder to the lifting platform in the powder feeding cylinder, thus completing the pre-powdering of the metal layer.
[0008] ② The lifting platform in the powder feeding cylinder continues to descend to a height of h2, and a single layer of diamond / metal matrix composite powder (such as Figure 2 The round roller moves from the printing cylinder to the powder feeding cylinder to cover the powder feeding cylinder with diamond / metal matrix composite powder, completing the pre-powdering of the diamond / metal matrix composite material layer, that is, completing the pre-laying of a slice A with a thickness of h0 (such as Figure 2 The state of the lower left corner area of the );
[0009] ③. Repeat the process of ① and ② to complete the pre-powdering of the entire powder feeding cylinder. After completion, the thickness of the powder in the powder feeding cylinder is N×h0, where N is a positive integer;
[0010] 3. ①, using the lifting platform in the powder feeding cylinder, the lifting platform in the printing cylinder and the round roller to deliver the uppermost diamond / metal matrix composite material layer with a thickness of h2 in the powder feeding cylinder to the printing cylinder, and print the diamond / metal matrix composite material layer to obtain the first layer of printing pattern;
[0011] ②, using the lifting platform in the powder delivery cylinder, the lifting platform in the printing cylinder and the round roller to deliver the topmost metal layer with a thickness of h1 in the powder delivery cylinder to the printing cylinder, and print the metal layer to obtain the second layer of printing pattern;
[0012] ③. Repeat the process of ① and ② to transfer all the powder in the powder feeding cylinder to the printing cylinder layer by layer and print layer by layer (see Figure 3 );
[0013] 4. Take out the printed part from the printing cylinder and perform post-processing on the printed part; utilize the density difference between the metal powder and the diamond / metal matrix composite material powder to separate the metal powder and the diamond / metal matrix composite material powder by heavy liquid, and wash, dry and recycle the two separated powders respectively;
[0014] The density of the heavy liquid is between the density of the metal and the density of the diamond / metal matrix composite material, and the two powders are separated by precipitation and floating of the powders.
[0015] The diamond / metal matrix composite material powder described in the present invention is diamond\copper (aluminum and other materials) containing an intermediate coating (an intermediate coating produced by plating Ti, W, Cr, Mo and other materials);
[0016] The most critical feature of the present invention is that in step 3, a diamond / metal matrix composite powder layer is printed by laser for the first time to form a skeleton, and then the metal layer printed above is melted to perform secondary densification on the skeleton (printed diamond / metal matrix composite powder layer) below, thereby obtaining a high-density print (see Figure 4 ).
[0017] The beneficial effects of the present invention are:
[0018] The present invention obtains a high-density printed part (the density of the product after step three reaches 93% to 96%) through secondary densification of the metal layer in situ, thereby ensuring the density of the diamond / metal-based composite material and giving full play to the advantages of 3D printing in the forming of complex structural parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a process flow chart of the present invention;
[0020] Figure 2 It is a schematic flow diagram of part of the process in step 2 of the present invention;
[0021] Figure 3 It is a schematic flow diagram of part of the process in step three of the present invention;
[0022] Figure 4 It is a schematic diagram of the principle of part of the process in step three of the present invention;
[0023] Figure 5 This is the SEM image of the print after processing in step 4 of experiment 2. DETAILED DESCRIPTION
[0024] Specific implementation method 1: This implementation method is a SLM high-density diamond metal-based composite printing method, which is specifically carried out according to the following steps:
[0025] 1. Establish a CAD model of the printed part, slice the CAD model, and obtain a slice A with a required layer thickness of h0; set the thickness of the metal layer powder material layer to h1, and the thickness of the diamond / metal matrix composite material layer to h2, and h0=h1+h2;
[0026] 2. ①. Fill the lifting platform in the printing cylinder with metal powder, and the lifting platform in the powder feeding cylinder is in a blank state and is located at the highest point in the powder feeding cylinder; raise the lifting platform in the printing cylinder to a height of h1, and lower the lifting platform in the powder feeding cylinder to a height of h1. The round roller of the printer moves from the printing cylinder to the powder feeding cylinder to feed the metal powder with a height of h1 in the original printing cylinder to the lifting platform in the powder feeding cylinder, completing the pre-powdering of the metal layer;
[0027] ② The lifting platform in the powder feeding cylinder continues to descend to a height of h2, and the diamond / metal matrix composite material powder required for a single layer is placed in the transition area between the printing cylinder and the powder feeding cylinder. The circular roller moves from the printing cylinder to the powder feeding cylinder to cover the diamond / metal matrix composite powder in the powder feeding cylinder, completing the pre-powder laying of the diamond / metal matrix composite material layer, that is, completing the pre-laying of a slice A with a thickness of h0;
[0028] ③. Repeat the process of ① and ② to complete the pre-powdering of the entire powder feeding cylinder. After completion, the thickness of the powder in the powder feeding cylinder is N×h0, where N is a positive integer;
[0029] 3. ①, using the lifting platform in the powder feeding cylinder, the lifting platform in the printing cylinder and the round roller to deliver the uppermost diamond / metal matrix composite material layer with a thickness of h2 in the powder feeding cylinder to the printing cylinder, and print the diamond / metal matrix composite material layer to obtain the first layer of printing pattern;
[0030] ②, using the lifting platform in the powder delivery cylinder, the lifting platform in the printing cylinder and the round roller to deliver the topmost metal layer with a thickness of h1 in the powder delivery cylinder to the printing cylinder, and print the metal layer to obtain the second layer of printing pattern;
[0031] ③. Repeat the process of ① and ② to transfer all the powder in the powder feeding cylinder to the printing cylinder layer by layer and print layer by layer;
[0032] 4. Take out the printed part from the printing cylinder and perform post-processing on the printed part; utilize the density difference between the metal powder and the diamond / metal matrix composite material powder to separate the metal powder and the diamond / metal matrix composite material powder by heavy liquid, and wash, dry and recycle the two separated powders respectively;
[0033] The density of the heavy liquid is between the density of the metal and the density of the diamond / metal matrix composite material, and the two powders are separated by precipitation and floating of the powders.
[0034] Specific implementation method 2: This implementation method is different from the specific implementation method 1 in that: the h0 described in step 1 is 5 μm to 200 μm. The rest is the same as the specific implementation method 1.
[0035] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the particle size of the metal powder in step 2① is 5 μm to 200 μm. The rest is the same as specific implementation method 1 or 2.
[0036] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the material of the metal powder in step 2① is copper, aluminum, copper alloy or aluminum alloy. The rest is the same as specific embodiments 1 to 3.
[0037] Specific embodiment 5: This embodiment is different from specific embodiment 4 in that the particle size of the diamond / metal matrix composite material powder described in step 2② is 5 μm to 200 μm. Other aspects are the same as those of specific embodiment 4.
[0038] Specific embodiment 6: This embodiment is different from specific embodiment 5 in that the diamond / metal matrix composite material powder described in step 2② is diamond\copper, aluminum, copper alloy or aluminum alloy. The rest is the same as specific embodiment 5.
[0039] Specific implementation example 7: This implementation example is different from specific implementation example 6 in that: in step 3, the printing environment is inert gas to ensure that the oxygen content is less than 0.1%. Other aspects are the same as specific implementation example 6.
[0040] Specific embodiment 8: This embodiment is different from specific embodiment 7 in that the inert gas in step 3 is Ar gas or N2 gas. The rest is the same as specific embodiment 7.
[0041] Specific embodiment 9: This embodiment differs from specific embodiment 8 in that: in step 3, the air pressure during printing is 10mbar-20mbar, the laser power is 300W-500W, the scanning speed is 100mm / s-500mm / s, and the substrate heating temperature is 200℃-400℃. Others are the same as specific embodiment 8.
[0042] Specific embodiment 10: This embodiment differs from specific embodiment 9 in that the post-treatment described in step 4 is hot isostatic pressing, the hot isostatic pressing temperature is 400°C to 800°C, the pressure is 20MPa to 100MPa, the time is 3h, and the heating and cooling rates are both 5K / min. Others are the same as specific embodiment 9.
[0043] The present invention is verified by the following tests:
[0044] Experiment 1: This experiment is a SLM high-density diamond metal matrix composite printing method, which is specifically carried out in the following steps:
[0045] 1. Establish a CAD model of the print part, slice the CAD model, and obtain a slice A with a required layer thickness of h0 (150 μm); set the thickness of the copper alloy powder material layer to h1 (30 μm), and the thickness of the diamond / copper alloy composite material powder layer to h2 (120 μm);
[0046] 2. ①. Fill the lifting platform in the printing cylinder with copper alloy powder, and the lifting platform in the powder feeding cylinder is in a blank state and is located at the highest point in the powder feeding cylinder; raise the lifting platform in the printing cylinder to a height of h1 (30 μm), and lower the lifting platform in the powder feeding cylinder to a height of h1 (30 μm). The round roller of the printer moves from the printing cylinder to the powder feeding cylinder to feed the copper alloy powder with a height of h1 (30 μm) in the original printing cylinder to the lifting platform in the powder feeding cylinder to complete the pre-powdering of the metal layer; the particle size of the copper alloy powder is 20 μm;
[0047] ②, the lifting platform in the powder feeding cylinder continues to descend to a height of h2 (120μm), and the diamond / copper alloy composite material powder required for a single layer is placed in the transition area between the printing cylinder and the powder feeding cylinder. The round roller moves from the printing cylinder to the powder feeding cylinder to cover the diamond / copper alloy composite powder in the powder feeding cylinder, completing the pre-powdering of the diamond / copper alloy composite material layer, that is, completing the pre-laying of a slice A with a thickness of h0 (150μm); the particle size of the diamond / copper alloy composite material powder is 50μm;
[0048] ③. Repeat the process of ① and ② to complete the pre-powdering of the entire powder feeding cylinder. After completion, the thickness of the powder in the powder feeding cylinder is N×h0, where N is a positive integer;
[0049] 3. ①, using the lifting platform in the powder feeding cylinder, the lifting platform in the printing cylinder and the round roller to deliver the uppermost diamond / copper alloy composite material layer with a thickness of h2 (120 μm) in the powder feeding cylinder to the printing cylinder, and printing the diamond / copper alloy composite material layer to obtain the first layer of printing pattern;
[0050] ②, using the lifting platform in the powder feeding cylinder, the lifting platform in the printing cylinder and the round roller to deliver the top copper alloy layer with a thickness of h1 (30 μm) in the powder feeding cylinder to the printing cylinder, and print the copper alloy layer to obtain the second layer of printing pattern;
[0051] ③. Repeat the process of ① and ② to transfer all the powder in the powder feeding cylinder to the printing cylinder layer by layer and print layer by layer;
[0052] In step 3, the printing environment is an inert gas to ensure that the oxygen content is less than 0.08%, and the inert gas is Ar gas;
[0053] During printing in step 3, the air pressure is 16 mbar, the laser power is 400 W, the scanning speed is 300 mm / s, the printed layers are all scanned by stripe laser, the focusing diameter of the laser point on the powder bed surface is set to 60 μm, and the heating temperature of the tungsten substrate is 350 °C;
[0054] 4. Remove the printed part from the printing cylinder and perform post-processing on the printed part; take advantage of the density difference between the copper alloy powder and the diamond / copper alloy composite powder (the density of the copper alloy powder is about 8.9g / cm 3 The density of diamond / copper alloy composite material is about 3.5g / cm 3 ~3.7g / cm 3 ), separating the metal powder and the diamond / metal matrix composite material powder by heavy liquid, and washing, drying and recovering the two separated powders respectively;
[0055] The density of the heavy liquid is between the density of metal and the density of diamond / metal matrix composite material, and the two powders are separated by precipitation and floating of the powders; the Krelich liquid (density: 4.3 g / cm 3 ) and deionized water (density: 1g / cm 3 ) are mixed in a mass ratio of 10:1, and the density of the heavy liquid is 4g / cm 3 ;
[0056] The post-treatment described in step 4 is hot isostatic pressing, the temperature of hot isostatic pressing is 400° C., the pressure is 30 MPa, the time is 3 h, and the heating and cooling rates are both 5 K / min.
[0057] Experiment 2: This experiment is a SLM high-density diamond metal matrix composite printing method, which is specifically carried out in the following steps:
[0058] 1. Establish a CAD model of the print part, slice the CAD model, and obtain a slice A with a required layer thickness of h0 (100 μm); set the thickness of the copper alloy powder material layer to h1 (30 μm), and the thickness of the diamond / copper alloy composite material powder layer to h2 (70 μm);
[0059] 2. ①. Fill the lifting platform in the printing cylinder with copper alloy powder, and the lifting platform in the powder feeding cylinder is in a blank state and is located at the highest point in the powder feeding cylinder; raise the lifting platform in the printing cylinder to a height of h1 (30 μm), and lower the lifting platform in the powder feeding cylinder to a height of h1 (30 μm). The round roller of the printer moves from the printing cylinder to the powder feeding cylinder to feed the copper alloy powder with a height of h1 (30 μm) in the original printing cylinder to the lifting platform in the powder feeding cylinder to complete the pre-powdering of the metal layer; the particle size of the copper alloy powder is 10 μm;
[0060] ②, the lifting platform in the powder feeding cylinder continues to descend to a height of h2 (70μm), and the diamond / copper alloy composite material powder required for a single layer is placed in the transition area between the printing cylinder and the powder feeding cylinder. The round roller moves from the printing cylinder to the powder feeding cylinder to cover the diamond / copper alloy composite powder in the powder feeding cylinder, completing the pre-powdering of the diamond / copper alloy composite material layer, that is, completing the pre-laying of a slice A with a thickness of h0 (100μm); the particle size of the diamond / copper alloy composite material powder is 60μm;
[0061] ③. Repeat the process of ① and ② to complete the pre-powdering of the entire powder feeding cylinder. After completion, the thickness of the powder in the powder feeding cylinder is N×h0, where N is a positive integer;
[0062] 3. ①, using the lifting platform in the powder feeding cylinder, the lifting platform in the printing cylinder and the round roller to deliver the uppermost diamond / copper alloy composite material layer with a thickness of h2 (70 μm) in the powder feeding cylinder to the printing cylinder, and print the diamond / copper alloy composite material layer to obtain the first layer of printing pattern;
[0063] ②, using the lifting platform in the powder feeding cylinder, the lifting platform in the printing cylinder and the round roller to deliver the top copper alloy layer with a thickness of h1 (30 μm) in the powder feeding cylinder to the printing cylinder, and print the copper alloy layer to obtain the second layer of printing pattern;
[0064] ③. Repeat the process of ① and ② to transfer all the powder in the powder feeding cylinder to the printing cylinder layer by layer and print layer by layer;
[0065] In step 3, the printing environment is an inert gas to ensure that the oxygen content is less than 0.08%, and the inert gas is nitrogen;
[0066] During printing in step 3, the air pressure is 16 mbar, the laser power is 400 W, the scanning speed is 500 mm / s, the printed layers are all scanned by stripe laser, the focusing diameter of the laser point on the powder bed surface is set to 80 μm, and the heating temperature of the tungsten substrate is 350 °C;
[0067] 4. Remove the printed part from the printing cylinder and perform post-processing on the printed part; take advantage of the density difference between the copper alloy powder and the diamond / copper alloy composite powder (the density of the copper alloy powder is about 8.9g / cm 3 The density of diamond / copper alloy composite material is about 3.5g / cm 3 ~3.7g / cm 3 ), separating the metal powder and the diamond / metal matrix composite material powder by heavy liquid, and washing, drying and recovering the two separated powders respectively;
[0068] The density of the heavy liquid is between the density of metal and the density of diamond / metal matrix composite material, and the two powders are separated by precipitation and floating of the powders; the Krelich liquid (density: 4.3 g / cm 3 ) and deionized water (density: 1g / cm 3 ) are mixed in a mass ratio of 10:1, and the density of the heavy liquid is 4g / cm 3 ;
[0069] The post-treatment described in step 4 is hot isostatic pressing, the temperature of hot isostatic pressing is 500° C., the pressure is 30 MPa, the time is 3 h, and the heating and cooling rates are both 5 K / min.
[0070] The density of the product after step 3 of experiment 2 reached 93% to 94% (before post-treatment).
[0071] Figure 5 This is the SEM image of the printout after processing in step 4 of experiment 2. It can be seen that it has good density.
Claims
1. A method for printing a SLM high-density diamond metal-based composite material, characterized in that The SLM printing method of high-density diamond metal matrix composites is carried out in the following steps:
1. Establish a CAD model of the printed part, slice the CAD model, and obtain a slice A with a required layer thickness of h0; set the thickness of the metal layer powder material layer to h1, and the thickness of the diamond / metal matrix composite material layer to h2, and h0=h1+h2; 2. ①. Fill the lifting platform in the printing cylinder with metal powder, and the lifting platform in the powder feeding cylinder is in a blank state and is located at the highest point in the powder feeding cylinder; raise the lifting platform in the printing cylinder to a height of h1, and lower the lifting platform in the powder feeding cylinder to a height of h1. The round roller of the printer moves from the printing cylinder to the powder feeding cylinder to feed the metal powder with a height of h1 in the original printing cylinder to the lifting platform in the powder feeding cylinder, completing the pre-powdering of the metal layer; ② The lifting platform in the powder feeding cylinder continues to descend to a height of h2, and the diamond / metal matrix composite material powder required for a single layer is placed in the transition area between the printing cylinder and the powder feeding cylinder. The circular roller moves from the printing cylinder to the powder feeding cylinder to cover the diamond / metal matrix composite powder in the powder feeding cylinder, completing the pre-powder laying of the diamond / metal matrix composite material layer, that is, completing the pre-laying of a slice A with a thickness of h0; ③. Repeat the process of ① and ② to complete the pre-powdering of the entire powder feeding cylinder. After completion, the thickness of the powder in the powder feeding cylinder is N×h0, where N is a positive integer; 3. ①, using the lifting platform in the powder feeding cylinder, the lifting platform in the printing cylinder and the round roller to deliver the uppermost diamond / metal matrix composite material layer with a thickness of h2 in the powder feeding cylinder to the printing cylinder, and print the diamond / metal matrix composite material layer to obtain the first layer of printing pattern; ②, using the lifting platform in the powder delivery cylinder, the lifting platform in the printing cylinder and the round roller to deliver the topmost metal layer with a thickness of h1 in the powder delivery cylinder to the printing cylinder, and print the metal layer to obtain the second layer of printing pattern; ③. Repeat the process of ① and ② to transfer all the powder in the powder feeding cylinder to the printing cylinder layer by layer and print layer by layer; 4. Take out the printed part from the printing cylinder and perform post-processing on the printed part; utilize the density difference between the metal powder and the diamond / metal matrix composite material powder to separate the metal powder and the diamond / metal matrix composite material powder by heavy liquid, and wash, dry and recycle the two separated powders respectively; The density of the heavy liquid is between the density of the metal and the density of the diamond / metal matrix composite material, and the two powders are separated by precipitation and floating of the powders.
2. A method for printing a SLM high-density diamond metal-based composite material according to claim 1, characterized in that The h0 described in step 1 is 5 μm to 200 μm.
3. The method for printing a SLM high-density diamond metal-based composite material according to claim 1, characterized in that The particle size of the metal powder described in step 2① is 5 μm to 200 μm.
4. A method for printing a SLM high-density diamond metal-based composite material according to claim 3, characterized in that The material of the metal powder described in step 2① is copper, aluminum, copper alloy or aluminum alloy.
5. The method for printing a SLM high-density diamond metal-based composite material according to claim 1, characterized in that The particle size of the diamond / metal matrix composite material powder described in step 2② is 5 μm to 200 μm.
6. A method for printing a SLM high-density diamond metal-based composite material according to claim 5, characterized in that The diamond / metal matrix composite material powder described in step 2② is diamond\copper, aluminum, copper alloy or aluminum alloy.
7. The method for printing a SLM high-density diamond metal-based composite material according to claim 1, characterized in that In step 3, the printing environment is an inert gas to ensure that the oxygen content is less than 0.1%.
8. The method for printing a SLM high-density diamond metal matrix composite material according to claim 7, characterized in that The inert gas described in step 3 is Ar gas or N2 gas.
9. The method for printing a SLM high-density diamond metal-based composite material according to claim 7, characterized in that During printing in step 3, the air pressure is 10 mbar to 20 mbar, the laser power is 300 W to 500 W, the scanning speed is 100 mm / s to 500 mm / s, and the substrate heating temperature is 200° C. to 400° C.
10. The method for printing a SLM high-density diamond metal-based composite material according to claim 1, characterized in that The post-treatment described in step 4 is hot isostatic pressing, the temperature of hot isostatic pressing is 400°C to 800°C, the pressure is 20MPa to 100MPa, the time is 3h, and the heating and cooling rates are both 5K / min.
Citation Information
Cited By