Winding method of high-temperature superconducting coil containing inner joint and superconducting hybrid magnet

By using strips without insulating layer to wind on the cylindrical frame in the high-temperature superconducting magnet and heating and welding at the end, a high-temperature superconducting coil containing an inner joint is formed, which solves the insufficient current carrying capacity and poor thermal stability. The problem of efficient utilization and performance improvement has been achieved.

CN119049874AActive Publication Date: 2024-11-29HUAZHONG UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411321027.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-29
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

The existing high-temperature superconducting magnets have problems such as insufficient current carrying capacity, high cost, poor thermal stability and poor welding performance in production and application, especially the high complexity and high cost caused by the winding method of single long strips. And the insulating layer reduces heat transfer efficiency.

Method used

A strip without insulation layer is wound on the cylindrical frame, and end heat welding is performed through clamping mechanism and heating mechanism to form a high-temperature superconducting coil containing an inner joint, simplifying the welding process and improving utilization and performance stability.

Benefits of technology

It realizes efficient utilization of short strips, improves the current carrying capacity and thermal stability of the magnet, reduces production costs, ensures the reliability of the magnet and engineering current density, and simplifies the winding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049874A_ABST
    Figure CN119049874A_ABST
Patent Text Reader

Abstract

The invention discloses a winding method of a high-temperature superconducting coil containing an inner joint and a superconducting hybrid magnet, and belongs to the technical field of superconducting magnets. A cylindrical framework with an insulating winding surface is arranged, and a clamping mechanism and a heating mechanism which can be used for heating and welding the end part of a strip are correspondingly arranged; and the clamping mechanism and the heating mechanism are used for completing heating welding between the ends of the two strips which are not coated with the insulating layers, so that the multiple strips which are not coated with the insulating layers are wound on the insulating winding surface of the cylindrical framework in sequence, and the high-temperature superconducting coil with the inner connector is obtained. According to the coil winding method, the steps are simple and convenient, operation is convenient and fast, the requirement for winding the same magnet coil through different strips can be met, the superconducting hybrid coil with the inner connector is rapidly obtained, the structural reliability in the strip winding process is fully guaranteed, different application and test requirements are met, and the application range is wide. And the engineering current density and the thermal stability of the superconducting hybrid coil are ensured, and the method has relatively good practical value and economic value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of superconducting magnets, and in particular relates to a high-temperature superconducting coil winding method containing an inner joint and a superconducting hybrid magnet. Background Art

[0002] High-temperature superconducting magnets have broad application prospects in the fields of electric power industry, magnetic levitation transportation, basic physics research, and medical research due to their high critical temperature, high upper critical magnetic field, excellent mechanical properties and current carrying capacity.

[0003] In general, a superconducting magnet is composed of multiple superconducting coils, and a single superconducting coil is generally wound with a superconducting tape coated with an insulating layer. In order to make the high-temperature superconducting magnet have a better current carrying capacity, the superconducting coil is generally wound with a single superconducting tape with high uniformity. However, whether it is the first-generation high-temperature superconducting tape based on bismuth, the second-generation high-temperature superconducting tape based on yttrium, or the new high-temperature superconducting tape represented by magnesium diboride, the production of a single superconducting tape with long distance, high current carrying uniformity and structural integrity will significantly increase the complexity of the tape manufacturing process and production costs.

[0004] Moreover, the use of a single long strip to wind the superconducting coil does not have a high utilization rate for the short strip, which is not conducive to reducing the cost of superconducting magnets and affects their further promotion and application. Although the use of superconducting joint manufacturing process to weld long-distance high-uniformity strips can reduce the demand for long strips in magnets to a certain extent, the joint resistance and mechanical strength will be affected by the welding material, and parameters such as the length of the joint area and the welding thickness will also restrict the performance of the long strip.

[0005] In addition, affected by the manufacturing process and material properties, the quench propagation speed of high-temperature superconducting tapes is slow, and the presence of the insulating layer significantly reduces the heat transfer efficiency between the tapes, making the thermal stability of the superconducting magnet poor, and also increasing the outer diameter of the superconducting magnet and reducing the engineering current density. When special working conditions such as local hot spots or local quenching occur, the heat inside the magnet cannot be effectively transferred from the inside of the superconducting magnet to the cooling medium, which leads to an increase in temperature rise. In severe cases, the magnet will be quenched or even damaged as a whole. Summary of the invention

[0006] In response to one or more of the above defects or improvement needs in the prior art, the present invention provides a high-temperature superconducting coil winding method containing an inner joint and a superconducting hybrid magnet, which can effectively realize the application of short strips in the magnet manufacturing process, reduce the impact of strip welding on the magnet performance, and ensure the reliability and stability of the magnet during use.

[0007] To achieve the above object, one aspect of the present invention provides a method for winding a high temperature superconducting coil containing an inner joint, which comprises the following steps: (1) Preparing a first strip material and a second strip material without an insulating layer, and a cylindrical skeleton with an insulating winding surface; (2) fixing the head end of the first strip on the insulating winding surface of the cylindrical skeleton, and winding the first strip on the cylindrical skeleton until the first strip is about to be wound to the end; (3) A clamping mechanism and a heating mechanism are provided corresponding to the end welding process of the two strips, and solder is prepared; (4) aligning the end of the first strip with the beginning of the second strip in the strip thickness direction, and placing the solder between the two solder strips to form a portion to be welded; thereafter, clamping the portion to be welded by a clamping mechanism, and assembling the clamping mechanism to a heating mechanism, and completing the heating welding of the ends of the two strips by the heating mechanism; (5) Continue winding the first tape end and the second tape on the cylindrical frame until the second tape is wound to the end, completing the tape winding and obtaining a high-temperature superconducting coil containing an inner joint.

[0008] As a further improvement of the present invention, in process (1), the width of the first strip is the same as that of the second strip; and / or The first strip and the second strip have different thicknesses, different critical currents, different mechanical strengths and / or different bending radii.

[0009] As a further improvement of the present invention, in process (1), the cylindrical frame is made of low-temperature resistant insulating material; or, the cylindrical frame is made of stainless steel material and its surface is subjected to insulation treatment.

[0010] As a further improvement of the present invention, in process (2), a plurality of buckles are provided corresponding to the first strip coil formed after the first strip is wound; and / or, in process (5), after the winding of all strips is completed, a plurality of buckles are provided on the cylindrical frame corresponding to the mixed strip coil formed after all strips are wound; and The buckle is arranged along the radial direction of the cylindrical frame, one end of which is clamped on the inner wall surface of the cylindrical frame, and the other end passes over the corresponding coil formed by winding around the outer circumference of the cylindrical frame and is clamped on the outermost strip of the coil.

[0011] As a further improvement of the present invention, in process (3), the solder is a low-temperature solder having a melting point between 70° C. and 150° C.

[0012] As a further improvement of the present invention, in process (3), the clamping mechanism includes a first cover plate and a second cover plate, and the heating mechanism is a heating table that can be used to place the two cover plates; The heating temperature of the heating table is 100°C to 250°C; the width of the two cover plates is 4 to 5 times the width of the two strips, the thickness is 1.5 to 3 cm, and the length is 2 to 3 times the length of the strip area to be welded.

[0013] As a further improvement of the present invention, the clamping mechanism comprises two metal clamping blocks arranged opposite to each other, a heating device arranged corresponding to the two metal clamping blocks, and a plurality of pressure members arranged on the heating device; The heating device is formed with a receiving cavity having two ends passing through it, and the width of the receiving cavity corresponds to the width of the metal clamping block, so that the two stacked metal clamping blocks can be correspondingly embedded in the receiving cavity; and One end of the pressure piece is arranged opposite to the top of the stacked metal clamping blocks, and the other end thereof is movably connected to the heating device. The heating piece can be adjusted to apply a clamping force to the stacked metal clamping blocks, so that the two strips clamped between the two metal clamping blocks can be continuously applied with uniform force by a plurality of pressure pieces during the welding process.

[0014] As a further improvement of the present invention, in process (4), before forming the portion to be welded, a process of setting the solder on the welding surfaces of the two strips is also performed: The end of the first strip and the beginning of the second strip are placed on a heating mechanism with the surfaces to be welded facing upward, and the heating mechanism performs initial heating on the two strips; solder is placed on the two surfaces to be welded, and heating is stopped after the solder on the two surfaces to be welded is completely melted; after the solder on the surfaces of the two strips cools and solidifies, the surfaces to be welded on the two strips respectively covered with solder are aligned and stacked to form the parts to be welded.

[0015] As a further improvement of the present invention, in process (4), before the welding ends of the two strips are aligned, a deoxidation layer treatment is performed on the end faces of the two ends facing each other, and the deoxidation layer treatment process is completed using phosphoric acid.

[0016] Another aspect of the present invention provides a superconducting hybrid magnet containing an inner joint, which includes a frame and a plurality of high-temperature superconducting coils assembled on the frame; at least one of the plurality of high-temperature superconducting coils is wound using the method for winding a high-temperature superconducting coil containing an inner joint.

[0017] The above-mentioned improved technical features can be combined with each other as long as they do not conflict with each other.

[0018] In general, compared with the prior art, the above technical solution conceived by the present invention has the following beneficial effects: (1) The method for winding a high-temperature superconducting coil containing an inner joint of the present invention comprises providing a cylindrical skeleton with an insulating winding surface and correspondingly providing a clamping mechanism and a heating mechanism capable of heating and welding the ends of the strip, and utilizing the clamping mechanism and the heating mechanism to complete the heating and welding between the ends of two strips without insulation layer coating, thereby realizing that a plurality of strips without insulation layer coating are sequentially wound on the insulating winding surface of the cylindrical skeleton to obtain a high-temperature superconducting coil containing an inner joint; utilizing the method of the present invention can effectively realize the reasonable utilization of shorter strips, improve the utilization rate of the strips, meet the requirements of winding a magnet coil when a certain strip is not long enough under special circumstances, and fully ensure the performance stability of the strips after being wound into magnets.

[0019] (2) The method for winding a high-temperature superconducting coil containing an inner joint of the present invention effectively ensures the reliability of the magnet coil after the strip is wound by preferably setting the material and setting form of the cylindrical skeleton and correspondingly designing the structural form of the clamping mechanism and the heating mechanism, simplifies the welding process between different strips, ensures the welding quality of the strips, and improves the flexibility and functional stability of the magnet coil winding.

[0020] (3) The superconducting hybrid magnet of the present invention comprises a frame and a plurality of high-temperature superconducting coils assembled on the frame, and the frame comprises at least one high-temperature superconducting coil wound by the high-temperature superconducting coil winding method of the present invention. The preferred design of the high-temperature superconducting coil makes the structure of the magnet compact and the performance stable, which can effectively improve the utilization rate of the strip and the economy of the superconducting magnet, and improve the engineering current density and thermal stability of the superconducting magnet, reduce the attenuation of the current carrying performance caused by the damage of the strip, and fully ensure the comprehensive performance of the magnet.

[0021] (4) The method for winding a high-temperature superconducting coil containing an inner joint in the present invention has simple steps and is easy to operate. It can meet the needs of winding the same magnet coil with different tapes, quickly obtain a superconducting hybrid coil containing an inner joint, fully ensure the structural reliability during the tape winding process, meet different application and test requirements, ensure the engineering current density and thermal stability of the superconducting hybrid coil, and has good practical value and economic value. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 It is a schematic flow chart of a method for winding a high-temperature superconducting coil having an inner joint in an embodiment of the present invention; Figure 2 is a schematic diagram of winding a first tape in a high-temperature superconducting coil winding method according to an embodiment of the present invention; Figure 3 is a schematic diagram of the first tape being wound in the high-temperature superconducting coil winding method according to an embodiment of the present invention; Figure 4 It is a schematic structural diagram of a clamping mechanism and a heating mechanism for strip welding in one embodiment of the present invention; Figure 5 , Figure 6 is a schematic structural diagram of a clamping mechanism and a heating mechanism in another embodiment of the present invention; Figure 7 Schematic diagram of the coil structure when the second strip is wound in an embodiment of the present invention.

[0024] In all the drawings, the same reference numerals represent the same technical features, specifically: 1. First strip; 2. Second strip; 3. Cylindrical frame; 4. Buckle; 5. First cover plate; 6. Second cover plate; 7. Solder; 8. Heating table; 9. Metal clamp; 10. Heating device; 11. Pressurizing member. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0026] In the description of the present invention, it should be understood that, unless otherwise expressly specified and limited, the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like to indicate orientations or positional relationships are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0027] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0028] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0029] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0030] Example: The high-temperature superconducting coil winding method in the preferred embodiment is mainly used for winding a high-temperature superconducting coil containing an inner joint, so as to obtain a high-temperature superconducting coil with a certain overcurrent capacity and self-protection capability.

[0031] like Figure 1 As shown in the figure, the method for winding a high-temperature superconducting coil containing an inner joint in a preferred embodiment of the present invention includes the following process: (1) Preparing materials, including a first strip material 1 without an insulating layer, a second strip material 2, and a cylindrical skeleton 3 with an insulating winding surface; Specifically, the reason why the first strip 1 and the second strip 2 without the insulating layer are used in the preferred embodiment is that removing the insulating layer can increase the engineering current density of the magnet and make the magnet structure more compact. At the same time, the wound strips are directly in contact with each other through the metal layer, the heat transfer speed is faster, and the thermal stability of the magnet is better. Moreover, since the overcurrent inside the strip can be shunted to the adjacent strip through the metal contact layer, the magnet has a certain overcurrent capacity and self-protection ability, so that the performance of the wound magnet is more excellent.

[0032] Furthermore, the coil winding method in the preferred embodiment does not have strict requirements on the uniformity of the tape. It can use high-temperature or low-temperature superconducting tapes with different current-carrying properties, mechanical strength and manufacturing processes to make joints according to application requirements, and then wind superconducting hybrid coils.

[0033] In actual material preparation, the width of the first tape 1 without an insulating layer is preferably kept consistent with the width of the second tape 2. At the same time, superconducting tapes with different thicknesses, different critical currents, and different mechanical strengths can be selected according to application requirements.

[0034] For example, in a specific preferred embodiment, the first tape 1 used for winding the inner coil is a superconducting tape with a small bending radius, and the second tape 2 used for winding the outer coil is a superconducting tape with a large bending radius.

[0035] In another specific preferred embodiment, the thickness of the second strip 2 is greater than the thickness of the first strip 1 .

[0036] In more detail, the cylindrical skeleton 3 in the preferred embodiment is preferably cylindrical, and the circumferential surface of the cylinder for winding the first strip 1 is an insulating surface.

[0037] Further preferably, the cylindrical skeleton 3 is made of low-temperature resistant insulating material, such as epoxy resin, ceramic or aluminum nitride material, etc.; or, the cylindrical skeleton 3 is made of stainless steel material and its surface is subjected to insulation treatment.

[0038] (2) Fixing the head end of the first strip 1 on the insulating winding surface of the cylindrical skeleton 3, and winding the first strip 1 on the cylindrical skeleton 3 until the first strip 1 is about to be wound to the end; In actual configuration, a driving device, such as a reduction motor, is provided corresponding to the winding of the cylindrical skeleton 3 . The cylindrical skeleton 3 is driven to rotate by the driving device to complete the winding process of the first strip 1 .

[0039] In more detail, in the preferred embodiment, the running speed of the first strip 1 is 0.1 m / min.

[0040] Of course, it is understandable that, according to the requirements of the setting, the winding of the first strip 1 can also be completed by other means and equipment, such as setting a tape reel to wind the first strip 1 .

[0041] By winding the first strip 1 on the cylindrical frame 3, a first coil can be formed on the outer periphery of the cylindrical frame 3. Figure 2 as shown in .

[0042] More preferably, after the winding of the first strip 1 is completed, the corresponding first coil is also provided with a plurality of buckles 4, which are preferably arranged along the radial direction of the cylindrical skeleton 3, with one end being clamped on the inner wall surface of the cylindrical skeleton 3, and the other end passing over the first coil on the outer periphery of the cylindrical skeleton 3 and being clamped on the outermost strip of the first coil.

[0043] For example, in Figure 3 In the preferred embodiment shown in , the number of buckles 4 arranged in the circumferential direction is 8, and each buckle 4 is further preferably arranged at equal intervals in the circumferential direction, so as to ensure the reliability of maintaining the winding state of each area position in the circumferential direction of the first coil.

[0044] Further preferably, during actual winding, the unwound end length of the first strip 1 is preferably not less than 50 mm, so as to facilitate subsequent strip processing steps and thereby meet the requirements of subsequent strip welding.

[0045] (3) A clamping mechanism and a heating mechanism are provided corresponding to the end welding process of the two strips, and solder 7 is prepared; In a preferred embodiment, the solder 7 is preferably a low-temperature solder having a melting point between 70°C and 150°C, such as Wood's alloy having a melting point between 100°C. The reason for choosing the low-temperature solder is that it has a low melting point and has little effect on the current carrying performance of the superconducting tape during the heat treatment process. Moreover, the residual amount of the low-temperature solder is small, and it is not easy to make the joint resistance too high due to the excessive thickness of the solder in the joint area.

[0046] During the actual welding operation, the amount of solder 7 used should be enough to completely cover the surface of one side of the two strips without dripping. If there is excessive solder, it is preferred to use a scraper to scrape the excess solder 7 to the edges of the two strips, and then use a solder absorber to absorb the excess solder 7.

[0047] Furthermore, the clamping mechanism in the preferred embodiment is used to clamp and fix the ends of the two strips with the solder 7 disposed between the end faces, so as to ensure that the ends of the two strips and the solder 7 can remain in the aligned state after the end alignment is completed.

[0048] Correspondingly, the heating mechanism is arranged corresponding to the clamping mechanism, and is used to heat the two strips to be welded, thereby melting the solder 7 between the two strips, thereby completing the welding of the two strips.

[0049] In a specific preferred embodiment, the clamping mechanism is preferably as follows Figure 4 The two cover plates shown in the figure are the first cover plate 5 and the second cover plate 6; accordingly, the heating mechanism is a heating table 8 provided corresponding to the two cover plates, and the heating temperature thereof is preferably 100°C to 250°C.

[0050] During the final welding, the first cover plate 5 is set on the heating table 8. Through the combination of the heating table 8 and the two cover plates, after the two cover plates complete the clamping setting of the two strips, the heating table 8 can heat and increase the temperature accordingly, thereby realizing the melting of the solder 7 and the welding of the ends of the two strips.

[0051] More preferably, the two cover plates are preferably copper cover plates, which have high thermal conductivity and can fully utilize the heat released by the heating platform 8 to accurately complete the melting and welding process of the solder 7 and ensure the welding quality of the low-temperature solder.

[0052] In actual use, the time for heating and welding using the heating table 8 is preferably 30 seconds to 90 seconds.

[0053] Further preferably, the two cover plates are of the same size and preferably have a rectangular plate structure, with a width of 4 to 5 times the width of the strip, a thickness of 1.5 to 3 cm, and a length of 2 to 3 times the length of the strip area to be welded.

[0054] In another specific preferred embodiment, the clamping mechanism and the heating mechanism are combined to form a hot pressing mechanism, which is arranged in the form of Figure 5 , Figure 6 As shown in the figure, it includes two metal clamping blocks 9 arranged opposite to each other, a heating device 10 arranged corresponding to the two metal clamping blocks 9, and a plurality of pressurizing members 11 arranged on the heating device 10.

[0055] Specifically, the heating device 10 in this embodiment is formed with a receiving cavity with two ends passing through, and the strip to be heated can be inserted into and placed in the receiving cavity. In actual setting, the width of the receiving cavity is preferably corresponding to the width of the metal clamp 9, so that the two stacked metal clamps 9 can be embedded in the receiving cavity. At the same time, one end of the pressure member 11 is set directly opposite to the top of the stacked metal clamp 9, and the other end thereof is movably connected to the heating device 10, and the clamping force can be applied to the stacked metal clamp 9 by adjusting the heating member 11.

[0056] Correspondingly, the first strip 1 and the second strip 2 whose ends overlap each other and with solder 7 arranged therebetween can be placed just between the two metal clamps 9, and during the welding process of the two strips, a plurality of pressure members 11 continuously apply a uniform force to the two strips to ensure the uniformity of the distribution of the welding material between the two strips and improve the welding effect of the strips.

[0057] In actual operation, the force uniformly applied by the pressure member 11 is 1 MPa to 10 MPa.

[0058] After the heating and welding of the strips are completed, a cooling mechanism, such as a hair dryer, may be further preferably provided. The provision of the cooling mechanism can be used to achieve rapid cooling of the clamping mechanism and the welding portion of the two strips.

[0059] (4) Aligning the end of the first strip 1 and the beginning of the second strip 2 in the strip thickness direction, and placing solder 7 between the two strips to form a portion to be welded; thereafter, clamping the portion to be welded by a clamping mechanism, and assembling the clamping mechanism to a heating mechanism, and completing the heating welding of the ends of the two strips by the heating mechanism; Furthermore, in actual operation, it is preferred that before forming the portion to be welded, a process of setting the solder 7 on the welding surfaces of the two strips is also performed: The end of the first strip 1 and the beginning of the second strip 2 are placed on a heating mechanism with the surfaces to be welded facing upward, and the two strips are initially heated by the heating mechanism; solder 7 is placed on the two surfaces to be welded, and heating is stopped after the solder on the two surfaces to be welded is completely melted; after the solder on the surfaces of the two strips cools and solidifies, the surfaces to be welded on the two strips, which are respectively covered with solder 7, are aligned and stacked to form a portion to be welded.

[0060] It is understood that after the solder 7 is covered on the two surfaces to be welded, the excess solder 7 can be scraped off to ensure the accuracy of the subsequent alignment of the two strips. At the same time, after the secondary heating and welding after the alignment of the two strips, the overflowed solder 7 can be further scraped off to ensure the cleanliness of the welding part.

[0061] Furthermore, during actual welding, before the two ends of the strip are stacked, it is preferred that the ends facing each other be subjected to a deoxidation treatment, and it is further preferred that the oxide layer on the end surface of the strip to be welded be removed by using an appropriate amount of phosphoric acid.

[0062] More preferably, the lengths of the first strip 1 and the second strip 2 subjected to the oxidation layer removal treatment are preferably the same.

[0063] (5) Continue winding the end of the first tape 1 and the second tape 2 on the cylindrical frame 3 until the second tape 2 is wound to the end, completing the winding of a single single-cake coil and obtaining a high-temperature superconducting coil with an inner joint.

[0064] In actual operation, after the second strip 2 is wound, the third, fourth, ... Nth strip (N is greater than 2) can be wound as needed to obtain a single-piece coil containing multiple (more than 2) strips.

[0065] In addition, after all the strips are wound, it is further preferred to set a plurality of buckles 4 on the cylindrical frame 3 corresponding to the wound coils, such as Figure 7 As shown in , the setting stability of the coils formed after each strip is wound is ensured.

[0066] By means of the aforementioned high-temperature superconducting coil winding method with an inner joint, it is possible to achieve a combination of superconducting tapes with different current carrying capacities and different mechanical strengths, and meet the requirements of strong field critical current testing, optimal design of thermal stability, optimal design of structural stability, etc. Moreover, the above method is also particularly suitable for the testing process of new tapes. Since the output of new tapes may be very small, and thus the coils cannot be completely wound, it is difficult to test the current carrying capacity and mechanical properties of the coils wound with new superconducting tapes. At this time, by using the method in the preferred embodiment, the new tapes and other types of tapes can be mixed and wound to complete the test.

[0067] As another aspect of the present invention, a superconducting hybrid magnet containing an inner joint is provided, which comprises a frame and a plurality of high-temperature superconducting coils assembled on the frame; and at least one of the plurality of high-temperature superconducting coils is wound using the aforementioned method for winding a high-temperature superconducting coil containing an inner joint.

[0068] As follows, the method in the preferred embodiment is specifically described through a specific embodiment, which relates to a yttrium barium copper oxide (YBCO)-iron selenium tellurium (FeSeTe) hybrid magnet and a winding method thereof, comprising the following steps: (1) preparing a FeSeTe strip without an insulating layer, a YBCO strip without an insulating layer, and an insulating frame made of epoxy resin; Specifically, the FeSeTe tape has a length of 0.5 m, a width of 5 mm, and a thickness of 0.15 mm; the YBCO tape has a length of 2.5 m, a width of 5 mm, and a thickness of 0.1 mm.

[0069] Correspondingly, the length of the insulating frame is 10 mm, the inner diameter is 25 mm, and the outer diameter is 30 mm, that is, the wall thickness of the insulating frame is 5 mm.

[0070] (2) Fix the head end of the FeSeTe tape on the outer wall of the insulating frame, and assemble the insulating frame on the rotating output shaft of the reduction motor, and control the FeSeTe tape to be wound at a tape speed of 0.1 m / min until the FeSeTe tape is wound to the tail end; Afterwards, the power supply of the reduction motor is turned off, and a number of clips are used to fix the coil wound by the FeSeTe tape around the outer periphery of the insulating frame.

[0071] (3) Prepare two copper plates as a clamping mechanism for welding the two strips, and set a heating table corresponding to the two copper plates; In actual operation, the two copper plates have the same size, with a width of 50 mm, a length of 150 mm, and a thickness of 10 mm.

[0072] (4) Use a small amount of phosphoric acid to remove the surface oxide layer on the end of the FeSeTe strip and the head of the YBCO strip, and remove the oxide layer on the end faces of the two strips to be welded; in actual operation, the length of the end faces of the two strips where the oxide layer is removed is 40 mm; The surface treated FeSeTe strip and YBCO strip are placed on the heating table 8 respectively, and the end faces after the oxidation layer treatment are facing upwards. Thereafter, a small amount of low-temperature solder is placed on the two end faces respectively, and each strip is heated by the heating table 8 until each low-temperature solder is completely melted; thereafter, the heating of the heating table 8 is stopped, so that the melted low-temperature solder solidifies and is evenly coated on the end faces to be welded of the two strips. Thereafter, the first copper plate, the end of the FeSeTe strip coated with low temperature solder, the head of the YBCO strip coated with low temperature solder, and the second copper plate are sequentially stacked on the heating table 8, so that the end faces of the two strips without the oxide layer are aligned with each other and clamped by the two copper plates; thereafter, the heating table 8 is controlled to perform secondary heating on the two strips stacked between the two copper plates to complete the end welding between the two strips. Thereafter, the heating table 8 is stopped, and the welding parts of the two strips are cooled to complete the welding of the ends of the two strips.

[0073] After welding is completed, it is further preferred to scrape off the welding material overflowing from the welding position of the two strips.

[0074] In this embodiment, the model of low-temperature solder selected is preferably HT100 Wood's alloy, which has a melting point of 100°C; the working temperature of the heating table 8 is controlled to 125°C, the initial heating time is 30s, the secondary heating time is 40s, and the cooling time after welding is completed is preferably 10min.

[0075] (5) Remove the clips on the insulating frame used to fix the wound coil 6, and continue to wind the YBCO tape until its end, so as to obtain a high-temperature superconducting coil made of two tapes and having an internal joint, thereby meeting the testing requirements of FeSeTe tape or YBCO tape.

[0076] The method for winding a high-temperature superconducting coil containing an inner joint in the present invention has simple steps and convenient operation, can meet the demand of winding the same magnet coil with different strips, quickly obtain a superconducting hybrid coil containing an inner joint, fully ensure the structural reliability during the strip winding process, meet different application and test requirements, ensure the engineering current density and thermal stability of the superconducting hybrid coil, and has good practical value and economic value.

[0077] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for winding a high-temperature superconducting coil containing an inner joint, characterized in that: The process includes the following: (1) Preparing a first strip material and a second strip material without an insulating layer, and a cylindrical skeleton with an insulating winding surface; (2) fixing the head end of the first strip on the insulating winding surface of the cylindrical skeleton, and winding the first strip on the cylindrical skeleton until the first strip is about to be wound to the end; (3) A clamping mechanism and a heating mechanism are provided corresponding to the end welding process of the two strips, and solder is prepared; (4) aligning the end of the first strip with the beginning of the second strip in the strip thickness direction, and placing the solder between the two solder strips to form a portion to be welded; thereafter, clamping the portion to be welded by a clamping mechanism, and assembling the clamping mechanism to a heating mechanism, and completing the heating welding of the ends of the two strips by the heating mechanism; (5) Continue winding the first tape end and the second tape on the cylindrical frame until the second tape is wound to the end, completing the tape winding and obtaining a high-temperature superconducting coil containing an inner joint.

2. The method for winding a high-temperature superconducting coil containing an inner connector according to claim 1, characterized in that: In process (1), the first strip and the second strip have the same width; and / or The first strip and the second strip have different thicknesses, different critical currents, different mechanical strengths and / or different bending radii.

3. The method for winding a high-temperature superconducting coil containing an inner connector according to claim 1, characterized in that: In process (1), the cylindrical frame is made of low-temperature resistant insulating material; or, the cylindrical frame is made of stainless steel material and its surface is subjected to insulation treatment.

4. The method for winding a high temperature superconducting coil containing an inner joint according to any one of claims 1 to 3, characterized in that: In process (2), a plurality of buckles are provided corresponding to the first strip coil formed after the first strip is wound; and / or, in process (5), after all strips are wound, a plurality of buckles are provided on the cylindrical frame corresponding to the mixed strip coil formed after all strips are wound; and The buckle is arranged along the radial direction of the cylindrical frame, one end of which is clamped on the inner wall surface of the cylindrical frame, and the other end passes over the corresponding coil formed by winding around the outer circumference of the cylindrical frame and is clamped on the outermost strip of the coil.

5. The method for winding a high temperature superconducting coil containing an inner joint according to any one of claims 1 to 3, characterized in that: In process (3), the solder is a low-temperature solder having a melting point between 70°C and 150°C.

6. The method for winding a high-temperature superconducting coil containing an inner connector according to claim 5, characterized in that: In process (3), the clamping mechanism includes a first cover plate and a second cover plate, and the heating mechanism is a heating table that can be used to place the two cover plates; The heating temperature of the heating table is 100°C to 250°C; the width of the two cover plates is 4 to 5 times the width of the two strips, the thickness is 1.5 to 3 cm, and the length is 2 to 3 times the length of the strip area to be welded.

7. The method for winding a high-temperature superconducting coil containing an inner connector according to claim 5, characterized in that: The clamping mechanism comprises two metal clamping blocks arranged opposite to each other, a heating device arranged corresponding to the two metal clamping blocks, and a plurality of pressure members arranged on the heating device; The heating device is formed with a receiving cavity having two ends passing through it, and the width of the receiving cavity corresponds to the width of the metal clamping block, so that the two stacked metal clamping blocks can be correspondingly embedded in the receiving cavity; and One end of the pressure piece is arranged opposite to the top of the stacked metal clamping blocks, and the other end thereof is movably connected to the heating device. The heating piece can be adjusted to apply a clamping force to the stacked metal clamping blocks, so that the two strips clamped between the two metal clamping blocks can be continuously applied with uniform force by a plurality of pressure pieces during the welding process.

8. The method for winding a high temperature superconducting coil containing an inner joint according to any one of claims 1 to 3, 6 and 7, characterized in that: In process (4), before forming the portion to be welded, a process of setting the solder on the welding surfaces of the two strips is also carried out: The end of the first strip and the beginning of the second strip are placed on a heating mechanism with the surfaces to be welded facing upward, and the heating mechanism performs initial heating on the two strips; solder is placed on the two surfaces to be welded, and heating is stopped after the solder on the two surfaces to be welded is completely melted; after the solder on the surfaces of the two strips cools and solidifies, the surfaces to be welded on the two strips respectively covered with solder are aligned and stacked to form the parts to be welded.

9. The method for winding a high-temperature superconducting coil containing an inner connector according to claim 8, characterized in that: In process (4), before the welding ends of the two strips are aligned, the two surfaces to be welded are subjected to a deoxidation treatment, wherein the deoxidation treatment is performed using phosphoric acid.

10. A superconducting hybrid magnet with an inner joint, comprising a frame and a plurality of high-temperature superconducting coils assembled on the frame; characterized in that: At least one of the plurality of high-temperature superconducting coils is wound using the method for winding a high-temperature superconducting coil containing an inner joint according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • A method for winding a high-temperature superconducting magnet

    CN109166725A

  • High-temperature superconducting coil heating wet winding device and winding method and system thereof

    CN114927339A

  • High temperature superconducting coil device and high temperature superconducting magnet device

    JP2019062005A

  • Superconducting coil and superconducting coil device

    JP2022021490A

  • Defect-irrelevant high temperature superconductor (HTS) magnet

    US20190074119A1