A method for preparing graphene quantum dots using heterogeneous catalyst

By using the reaction of manganese dioxide with water and graphene oxide, combined with hydrochloric acid to convert manganese ions, the problem of difficult control of the heat-induced Fenton reaction is solved, and graphene quantum dots without ultraviolet irradiation, simple devices, and no impurities introduced are realized. Preparation ensures the stability of the reaction and the purity of the product.

CN115924896BActive Publication Date: 2024-10-22SHANGHAI NAT ENG RES CENT FORNANOTECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211674694.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-10-22
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

The heat-induced Fenton reaction is difficult to control, causing graphene quantum dots to continue to react to generate carbon dioxide and water after they are generated, and cannot stay at the stage of generating graphene quantum dots.

Method used

Use heterogeneous catalyst manganese dioxide and water to stir vigorously, add hydrogen peroxide and neutral graphene oxide solution, convert manganese dioxide into manganese (II) ions through hydrochloric acid, filter and dialyze to obtain graphene quantum dots.

Benefits of technology

It realizes that no UV light irradiation is required, the device is simple, the product is easy to handle and no new impurities are introduced, the reaction process is controlled by graphene quantum dots, autocatalysis is avoided, and the stability of the generated graphene quantum dots is ensured.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing graphene quantum dots using a heterogeneous catalyst, wherein manganese dioxide particles are dispersed in water and stirred vigorously; stirring is maintained, the obtained dispersion is boiled, heating is stopped and hydrogen peroxide is added; a neutral graphene oxide solution is immediately added to the obtained reaction solution and stirring is continued, hydrogen peroxide is appropriately added while the solution is kept slightly boiling; heating is stopped, stirring is continued, hydrochloric acid and hydrogen peroxide are added to convert all manganese dioxide into manganese (II) ions; the obtained reaction solution is filtered, and the obtained liquid is dialyzed to obtain graphene quantum dots. Advantages of the invention The reaction does not require ultraviolet irradiation, and the device is simple. The product is easy to handle, and no new impurities are introduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of carbon nanomaterials, more specifically, to graphene quantum dots, and in particular to a method for preparing graphene quantum dots using a heterogeneous catalyst. Background Art

[0002] The Fenton reaction is a strong oxidation reaction with iron ions as catalyst and hydrogen peroxide as oxidant. It is often used for oxidation treatment of organic wastewater. Graphene quantum dots are small graphene sheets with lateral dimensions less than 100 nm. The photo-Fenton reaction induced by ultraviolet light can cut graphene oxide into graphene quantum dots (Zhou X, Zhang Y, Wang C, et al. Photo-Fenton reaction of graphene oxide: a new strategy to preparegraphene quantum dots for DNA cleavage[J]. ACS nano, 2012, 6(8): 6592-6599.). The reaction process is controlled by the intensity and time of ultraviolet light irradiation. The irradiation can be stopped at any time and the reaction will stop quickly. However, the Fenton reaction induced by heating without ultraviolet light irradiation cannot be used to produce graphene quantum dots, because the graphene quantum dots as the product can be combined with iron ions to form a complex with higher catalytic activity, which continuously accelerates the reaction, that is, the so-called autocatalytic phenomenon. Therefore, the thermally induced Fenton reaction generally cannot stop at the stage of producing graphene quantum dots, but will continue to react to produce carbon dioxide and water. Some manganese oxides can also trigger a strong oxidation reaction in hydrogen peroxide solution, which is called Fenton-like reaction (Ma Z, Wei X, Xing S, et al. Hydrothermal synthesis and characterization of surface-modified δ-MnO2 with high Fenton-like catalytic activity[J]. Catalysis Communications, 2015, 67:68-71.). Graphene quantum dots can also accelerate this type of heterogeneous Fenton-like reaction (Wu X, Zhang Y, Han T, et al. Composite of graphenequantum dots and Fe3O4 nanoparticles: peroxidase activity and application inphenolic compound removal[J]. Rsc Advances, 2013, 4(7):3299-3305.). However, when the content of graphene quantum dots increases, it can also shield the active sites on the surface of metal oxides to slow down the reaction, which provides a natural termination mechanism for the reaction without having to wait for a reactant to be exhausted. Summary of the invention

[0003] In view of the problem that the heat-induced Fenton reaction is difficult to control, the present invention aims to provide a method for preparing graphene quantum dots using a heterogeneous catalyst.

[0004] The present invention is implemented by the following scheme: A method for preparing graphene quantum dots using a heterogeneous catalyst comprises the following steps:

[0005] (1) Disperse manganese dioxide particles in water and stir vigorously.

[0006] (2) While maintaining stirring, boil the dispersion obtained in step (1), stop heating and add hydrogen peroxide.

[0007] (3) Immediately add the neutral graphene oxide solution to the reaction solution obtained in step (2) and continue stirring. Add hydrogen peroxide as appropriate.

[0008] (4) Continue stirring and add hydrochloric acid and hydrogen peroxide to convert all manganese dioxide into manganese (II) ions.

[0009] (5) Filter the reaction solution obtained in step (4), and dialyze the resulting liquid to obtain graphene quantum dots.

[0010] Preferably, in step (1), the manganese dioxide particles d 50 = 50 nm.

[0011] Preferably, the mass of graphene oxide added in step (3) is 5 times the mass of manganese dioxide added in step (1).

[0012] Advantages of the present invention:

[0013] (1) The reaction does not require ultraviolet light irradiation and the device is simple.

[0014] (2) The product is easy to handle and will not introduce new impurities.

[0015] The present invention utilizes the graphene quantum dots generated by the reaction to control the reaction process. In the initial stage of the reaction, the generated graphene quantum dots are compounded with manganese dioxide particles to accelerate the reaction. When the generated graphene quantum dots increase further, they cover the active sites on the surface of the manganese dioxide particles, which slows down the reaction and eventually stops. In the product treatment, hydrochloric acid is added to acidify the manganese dioxide so that the oxidizability is enhanced and it is smoothly reduced to divalent manganese ions. At this time, hydrogen peroxide is converted into oxygen as a reducing agent. Since manganese (II) ions are inevitably introduced during the preparation process of graphene oxide using the improved Hummers method, another advantage of the present method is that no new impurity ions are introduced. DETAILED DESCRIPTION

[0016] The present invention will be further described below in conjunction with specific examples. The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0017] Example 1.

[0018] . A method for preparing graphene quantum dots using a heterogeneous catalyst is prepared according to the following steps:

[0019] (1) 1 mg of manganese dioxide catalyst (d 50 = 50 nm) were dispersed in 50 mL and stirred vigorously;

[0020] (2) heating the dispersion obtained in step (1) under vigorous stirring until it boils, stopping heating, adding 0.2 mL of commercially available hydrogen peroxide (30%) into the solution with a plastic dropper, bringing to a boil, stopping heating and adding hydrogen peroxide;

[0021] (3) Disperse 5 mg of graphene oxide in 10 mL of water and add sodium hydroxide solution to neutralize it; immediately add the obtained neutral graphene oxide dispersion to the manganese dioxide dispersion obtained in step (2) which is close to boiling, keep stirring and heating to keep the solution slightly boiling, and add 0.2 mL of commercially available 30% hydrogen peroxide to the center of the solution with a dropper every 10 minutes, adding a total of 1.0 mL of hydrogen peroxide; then stop heating;

[0022] (4) Stop heating, continue stirring to allow the reaction to return to room temperature, add 1 mL of commercially available 36% concentrated hydrochloric acid, continue stirring, and add 0.1 mL of 30% hydrogen peroxide to convert all manganese dioxide into manganese (II) ions;

[0023] (5) Filter out the unreacted solids and dialyze the solution until it becomes neutral to obtain a graphene quantum dot solution.

[0024] The above embodiments are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for preparing graphene quantum dots using a heterogeneous catalyst, characterized in that: Prepare as follows: (1) 1 mg particle size d 50 = 50 nm manganese dioxide catalyst was dispersed in 50 mL and stirred vigorously; (2) heating the dispersion obtained in step (1) under vigorous stirring until it boils, stopping heating, adding 0.2 mL of commercially available 30% hydrogen peroxide into the solution with a plastic dropper, bringing to a boil, stopping heating and adding hydrogen peroxide; (3) Disperse 5 mg of graphene oxide in 10 mL of water and add sodium hydroxide solution to neutralize it to neutrality; immediately add the obtained neutral graphene oxide dispersion to the manganese dioxide dispersion obtained in step (2) which is nearly boiling, keep stirring and heating to keep the solution slightly boiling, and add 0.2 mL of commercially available 30% hydrogen peroxide to the center of the solution with a dropper every 10 minutes, and stop heating after adding a total of 1.0 mL of hydrogen peroxide; (4) Stop heating, continue stirring to allow the reaction to return to room temperature, add 1 mL of commercially available 36% concentrated hydrochloric acid, continue stirring, and add 0.1 mL of 30% hydrogen peroxide to convert all manganese dioxide into manganese II ions; (5) Filter out the unreacted solids and dialyze the solution until it becomes neutral to obtain a graphene quantum dot solution.