A method for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds

By adding polyisocyanate compounds and amine compounds to hydroxyl-containing polymer compounds for modification, the problem of poor compatibility between dinitramide ammonium and hydroxyl-containing polymer compounds was solved, and efficient coating and mechanical strength improvement were achieved, promoting application of green high-energy materials.

CN115926095BActive Publication Date: 2024-10-15XIAN MODERN CHEM RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211556461.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-10-15
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

Ammonium dinitramide has poor chemical compatibility with hydroxyl-containing polymer compounds, resulting in poor coating quality and high energy loss, making it impossible to realize the application of green high-energy materials.

Method used

By adding polyisocyanate compounds and amine compounds to hydroxyl-containing polymer compounds for modification, the compatibility of dinitramide ammonium and hydroxyl-containing polymer compounds is improved, and the modified hydroxyl-containing polymer material is used to coat dinitramide ammonium , improve its chemical compatibility and waterproof performance.

Benefits of technology

The chemical compatibility between ammonium dinitramide and hydroxyl-containing polymer compounds is significantly improved, the mechanical strength of the coating layer and solid particles is improved, energy loss is reduced, and the application of green high-energy materials is realized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115926095B_ABST
    Figure CN115926095B_ABST
Patent Text Reader

Abstract

The invention provides a method for improving the compatibility of ammonium dinitramide and a hydroxyl-containing polymer compound. The method achieves the change of the polymer hydroxyl group by reacting the polymer hydroxyl group with an isocyanate compound and then continuing to react with an amine substance. The chemical compatibility of ammonium dinitramide and the hydroxyl-containing polymer is improved by changing the hydroxyl group on the polymer. The method for improving the compatibility of ammonium dinitramide and the hydroxyl-containing polymer compound is helpful to use the hydroxyl-containing polymer compound in the propellant formula, and the modified hydroxyl-containing polymer material is used to coat the ammonium dinitramide, which is helpful to improve the hygroscopicity of the ammonium dinitramide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of energetic material interaction, relates to ammonium dinitramide and a hydroxyl-containing polymer compound, and specifically relates to a method for improving the compatibility of ammonium dinitramide and the hydroxyl-containing polymer compound. Background Art

[0002] Ammonium dinitramide is a high-energy, environmentally friendly high-energy material and an ideal substitute for ammonium perchlorate in propellants. Due to the hygroscopicity of ammonium dinitramide, its application is basically limited to liquid propellants. To solve the hygroscopicity problem of ammonium dinitramide, the current common method is to melt and granulate ammonium dinitramide and then coat it with a polymer to prevent it from absorbing moisture. However, this method is currently only reported in literature and has not been actually applied in engineering. The reason is that on the one hand, the coating quality of ammonium dinitramide is poor, the coating is incomplete, and the physical incompatibility between the coating layer and ammonium dinitramide leads to phase separation; on the other hand, the use of inert materials for coating leads to large energy loss, and it is impossible to achieve green high energy, which violates the original intention of using ammonium dinitramide.

[0003] Nitrocellulose is the main component of civilian nitrocellulose paint and is also commonly used as a coating to achieve moisture-proofing. Due to its excellent performance, nitrocellulose is an easily available industrial raw material and is also one of the commonly used components of propellants. In theory, it can be an ideal propellant coating material. However, existing studies have shown that ammonium dinitramide and nitrocellulose have strong interactions and poor chemical compatibility, which does not meet the requirements of formula design. It is generally recognized in the industry that nitrocellulose and ammonium dinitramide are difficult to coexist.

[0004] As a common component of composite propellants, polyethylene glycol has long been used in composite propellants. Polyethylene glycol itself is non-toxic and hydrophilic, and has good physical compatibility with ammonium dinitramide. During the melt granulation coating process, polyethylene glycol molecules can penetrate into the ammonium dinitramide particles, and a transition layer can be constructed between the waterproof layer of the coating layer and the ammonium dinitramide, thereby improving the mechanical strength of the coating layer and the solid particles. However, existing studies have shown that ammonium dinitramide and polyethylene glycol have strong interactions, poor chemical compatibility, and do not meet the requirements of formula design. Therefore, it is generally recognized in the industry that polyethylene glycol and ammonium dinitramide cannot be used together. Summary of the invention

[0005] In view of the defects and shortcomings of the prior art, the object of the present invention is to provide a method for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds, thereby solving the technical problem of poor chemical compatibility between hydroxyl-containing polymer compounds and ammonium dinitramide in the prior art.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:

[0007] A method for improving the compatibility of ammonium dinitramide and a hydroxyl-containing polymer compound, wherein the method uses a polyisocyanate compound to modify the hydroxyl-containing polymer compound to improve the compatibility of ammonium dinitramide and the hydroxyl-containing polymer compound; the hydroxyl-containing polymer compound is nitrocellulose or polyethylene glycol.

[0008] The method for modifying a hydroxyl-containing polymer compound comprises the following steps:

[0009] Step 1, adding a solvent to a hydroxyl-containing polymer compound, stirring while adding, shaking after adding, and standing after shaking to obtain a solution S1 after the hydroxyl-containing polymer compound is dissolved; the hydroxyl-containing polymer compound is nitrocellulose or polyethylene glycol;

[0010] Step 2, adding a polyisocyanate compound to the solution S1 obtained in step 1, and then adding a catalyst, and stirring to obtain a solution S2;

[0011] Step 3, heating and stirring the solution S2 obtained in step 2 to obtain a reaction solution S3;

[0012] Step 4: After the reaction solution S3 obtained in step 3 is cooled, an amine compound is added, and the reaction solution S4 is obtained after stirring. After the reaction solution S4 is allowed to stand and dry, a modified hydroxyl-containing polymer material is obtained.

[0013] The present invention also has the following technical features:

[0014] Specifically, the polyisocyanate compound is isophorone diisocyanate, toluene diisocyanate, 4,4'-diphenylmethane diisocyanate or hexamethylene diisocyanate.

[0015] Optionally, the method uses a monoisocyanate compound to modify the hydroxyl-containing polymer compound to improve the compatibility of ammonium dinitramide and the hydroxyl-containing polymer compound; the method specifically comprises the following steps:

[0016] Step 1, adding a solvent to a hydroxyl-containing polymer compound, stirring while adding, shaking after adding, and standing after shaking to obtain a solution S1 after the hydroxyl-containing polymer compound is dissolved; the hydroxyl-containing polymer compound is nitrocellulose or polyethylene glycol;

[0017] Step 2, adding a monoisocyanate compound to the solution S1 obtained in step 1, and then adding a catalyst, and stirring to obtain a solution S2;

[0018] Step 3, heating and stirring the solution S2 obtained in step 2 to obtain a reaction solution S3;

[0019] Step 4: The reaction solution S3 obtained in step 3 is allowed to stand and dry to obtain a modified hydroxyl-containing polymer material.

[0020] Specifically, the monoisocyanate compound is propyl isocyanate, hexyl isocyanate, benzyl isocyanate, octyl isocyanate or p-toluene isocyanate.

[0021] Specifically, the amine compound is hexamethylenediamine or ethylenediamine.

[0022] Specifically, the solvent is ethyl acetate, acetone or tetrahydrofuran.

[0023] Specifically, the catalyst is dibutyltin dilaurate or stannous octoate.

[0024] Specifically, in step 2, the stirring condition is: stirring at a speed of 100 rpm to 500 rpm for 0.5 h to 48 h.

[0025] Specifically, in step 3, the heating and stirring conditions are: in an oil bath at 25°C to 80°C, stirring at a constant temperature of 100rpm to 500rpm for 4h to 12h.

[0026] Specifically, in step 4, the conditions for standing and drying are: standing for 12 hours, and then vacuum drying at a temperature of 55° C. for 3 hours.

[0027] Specifically, the mass ratio of the monoisocyanate compound to the hydroxyl-containing polymer compound is (0.7-0.8):3.

[0028] Specifically, the mass ratio of the polyisocyanate compound, the amine compound and the hydroxyl-containing polymer compound is (1.2-1.9):(0.81-0.99):3.

[0029] The beneficial technical effects of the present invention compared with the prior art are as follows:

[0030] (I) The method of improving the compatibility of ammonium dinitramide with a hydroxyl-containing polymer compound of the present invention is to react the hydroxyl group of the polymer with an isocyanate compound and then react with an amine substance to achieve the change of the hydroxyl group of the polymer. By changing the hydroxyl group on the polymer, the chemical compatibility of ammonium dinitramide with the hydroxyl-containing polymer is improved.

[0031] (II) The method of improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds of the present invention is helpful for using hydroxyl-containing polymer compounds in propellant formulations, and the use of modified hydroxyl-containing polymer materials to coat ammonium dinitramide is helpful for improving the hygroscopicity of ammonium dinitramide.

[0032] (III) The method of improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds of the present invention has mild reaction conditions and simple operation, which is conducive to promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the process flow for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds.

[0034] Figure 2 This is a curve chart showing the change in the degassing pressure of the modified nitrocellulose material and ammonium dinitramide over time in Example 1.

[0035] Figure 3 This is a curve chart showing the change in the degassing pressure of the modified polyethylene glycol material and ammonium dinitramide over time in Example 1 in Example 4.

[0036] The meanings of the abbreviations of the symbols in the figure are: AND represents ammonium dinitramide, NC represents nitrocellulose, IPDI represents isophorone diisocyanate, HMDA represents hexamethylenediamine, TDI represents toluene diisocyanate, and PEG represents polyethylene glycol.

[0037] The technical solution of the present invention is further described below in conjunction with embodiments. DETAILED DESCRIPTION

[0038] The present invention is based on the many advantages of nitrocellulose and polyethylene glycol described in the background technology, and on the basis of studying the interaction mechanism between nitrocellulose and polyethylene glycol and ammonium dinitramide, a method for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymers is proposed.

[0039] It should be noted that all raw materials used in the present invention, unless otherwise specified, are raw materials known in the art, for example:

[0040] The nitrocellulose contains nitrocellulose with a nitrogen content of 6.76% to 14% as known in the prior art.

[0041] The polyethylene glycol used had a number average molecular weight of 800.

[0042] In accordance with the above technical scheme, specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical scheme of this application fall within the protection scope of the present invention.

[0043] Embodiment 1:

[0044] This embodiment provides a method for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds. The method uses a modified hydroxyl-containing polymer material to improve the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds. Figure 1 As shown, the method for modifying a hydroxyl-containing polymer compound comprises the following steps:

[0045] Step 1, weigh 3g of nitrocellulose, add 60g of ethyl acetate, stir with a glass rod during the addition, so that the nitrocellulose and ethyl acetate are fully in contact, accelerate the dissolution of the nitrocellulose, and shorten the dissolution time; then place it on an oscillating screen and oscillate for 1h. After the oscillation is completed, let it stand at room temperature for 12h. After the nitrocellulose is dissolved, a nitrocellulose solution S1 is obtained.

[0046] Step 2: Add 1.9 g of isophorone diisocyanate to the nitrocellulose solution S1 obtained in step 1, and then add 6 mg of dibutyltin diisocyanate, and stir at 200 rpm for 30 min to obtain solution S2. The amount of the isocyanate compound added is determined according to the amount of hydroxyl groups on the nitrocellulose, and the ratio of the N=C=O mole number of the isocyanate compound to the hydroxyl mole number of the nitrocellulose is generally 1 to 2.

[0047] Step 3: Place the solution S2 obtained in step 2 in an oil bath at 50° C. and stir at a constant temperature of 200 rpm for 4 hours to obtain a reaction solution S3.

[0048] Step 4, after the reaction solution S3 obtained in step 3 is cooled to room temperature, 0.99 g of hexamethylenediamine is added and stirring is continued for 20 min to obtain reaction solution S4, and then the reaction solution S4 is poured into a culture dish, and allowed to stand in a fume hood at room temperature for 12 h, and then vacuum dried in a vacuum oven at 55° C. for 3 h to obtain a modified nitrocellulose material.

[0049] Performance test of Example 1:

[0050] In this embodiment, the gas volume method was used to test the interaction and chemical compatibility between the modified nitrocellulose material and ammonium dinitramide. The specific process of the test is as follows:

[0051] First, 0.5 g of the modified nitrocellulose material after drying and removing the solvent and 0.5 g of ammonium dinitramide were weighed, mixed and placed in the first reaction tank; 0.5 g of unmodified nitrocellulose and 0.5 g of ammonium dinitramide were weighed, mixed and placed in the second reaction tank; 1.0 g of the modified nitrocellulose material after drying and removing the solvent was weighed and placed in the third reaction tank; 1.0 g of ammonium dinitramide was weighed and placed in the fourth reaction tank.

[0052] Then assemble the above four reaction cells into the reaction tube, connect the pressure sensor and the reaction tube with a pressure line, and tighten it to ensure that it is airtight; then place the reaction tube in a stable 100℃ constant temperature furnace, start heating, and record the pressure-time data at the same time. After heating for 40 hours, take out the reaction tube, and qualitatively judge the degree of interaction by the pressure change, and quantitatively judge the compatibility by the amount of gas released.

[0053] In this embodiment, the test results and evaluations are as follows:

[0054] like Figure 2As shown, the pressure of nitrocellulose and ammonium dinitramide isocyanate is much higher than that of modified nitrocellulose material and ammonium dinitramide, indicating that the interaction between modified nitrocellulose material and ammonium dinitramide is weak and the compatibility is good. The measured data were converted into the degassing volume under standard conditions, and the results are as follows: the degassing volume of modified nitrocellulose material is 0.44mL, the degassing volume of ammonium dinitramide is 0.65mL, the degassing volume of unmodified nitrocellulose and ammonium dinitramide is 23.68mL, and the degassing volume of modified nitrocellulose material and ammonium dinitramide is 0.81mL. From the degassing results, it can be seen that the chemical compatibility of modified nitrocellulose material and ammonium dinitramide is much better than that of unmodified nitrocellulose and ammonium dinitramide.

[0055] Embodiment 2:

[0056] This embodiment provides a method for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds, which uses modified hydroxyl-containing polymer materials to improve the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds. The method for modifying hydroxyl-containing polymer compounds includes the following steps:

[0057] Step 1, weigh 3g of nitrocellulose, add 60g of ethyl acetate, stir with a glass rod during the addition, so that the nitrocellulose and ethyl acetate are fully in contact, accelerate the dissolution of the nitrocellulose, and shorten the dissolution time; then place it on an oscillating screen and oscillate for 1h. After the oscillation is completed, let it stand at room temperature for 12h. After the nitrocellulose is dissolved, a nitrocellulose solution S1 is obtained.

[0058] Step 2: Add 0.72 g of isopropyl isocyanate to the nitrocellulose solution S1 obtained in step 1, and then add 6 mg of dibutyltin dilaurate, and stir at 200 rpm for 30 minutes to obtain solution S2.

[0059] Step 3: Place the solution S2 obtained in step 2 in an oil bath at 50° C. and stir at a constant temperature of 200 rpm for 4 hours to obtain a reaction solution S3.

[0060] Step 4: Pour the reaction solution S3 obtained in step 3 into a culture dish, let it stand in a fume hood at room temperature for 12 hours, and then dry it in a vacuum oven at 55° C. for 3 hours to obtain a modified nitrocellulose material.

[0061] Performance test of Example 2:

[0062] In this example, the gas volume method was used to test the interaction and chemical compatibility between the modified nitrocellulose material and ammonium dinitramide. It should be noted that in this example, the test results of ammonium dinitramide and unmodified nitrocellulose and ammonium dinitramide were all based on the test results in Example 1. The specific process of the test is as follows:

[0063] First, 0.5 g of the modified nitrocellulose material after drying and removing the solvent and 0.5 g of ammonium dinitramide were weighed, mixed and placed in the first reaction tank; 1.0 g of the modified nitrocellulose material after drying and removing the solvent was weighed and placed in the second reaction tank.

[0064] Then assemble the two reaction cells into the reaction tube, connect the pressure sensor and the reaction tube with a pressure line, and tighten to ensure airtightness; then place the reaction tube in a stable 100°C constant temperature furnace, start heating, and record the pressure-time data at the same time. After heating for 40 hours, take out the reaction tube, and qualitatively judge the degree of interaction by the pressure change, and quantitatively judge the compatibility by the amount of outgassing.

[0065] In this embodiment, the test results and evaluations are as follows:

[0066] The measured data were converted into the gas release under standard conditions, and the results were as follows: the gas release of the modified nitrocellulose material was 0.06 mL, the gas release of ammonium dinitramide was 0.65 mL, the gas release of the unmodified nitrocellulose and ammonium dinitramide was 23.68 mL, and the gas release of the modified nitrocellulose material and ammonium dinitramide was 1.37 mL. From the gas release results, it can be seen that the interaction between the modified nitrocellulose material and ammonium dinitramide is weak, and the chemical compatibility of the modified nitrocellulose material and ammonium dinitramide is much better than that of the unmodified nitrocellulose and ammonium dinitramide.

[0067] Embodiment 3:

[0068] This embodiment provides a method for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds, which uses modified hydroxyl-containing polymer materials to improve the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds. The method for modifying hydroxyl-containing polymer compounds includes the following steps:

[0069] Step 1, weigh 1g of polyethylene glycol, add 20g of ethyl acetate, stir with a glass rod during the addition, so that the polyethylene glycol and ethyl acetate are fully in contact, accelerate the dissolution of the polyethylene glycol, and shorten the dissolution time; then place it on an oscillating screen and oscillate for 0.5h. After the oscillation is completed, let it stand at room temperature for 12h. After the polyethylene glycol is dissolved, a polyethylene glycol solution S1 is obtained.

[0070] Step 2: Add 0.4 g of toluene diisocyanate to the polyethylene glycol solution S1 obtained in step 1, and then add 6 mg of dibutyltin diisocyanate, and stir at 200 rpm for 30 minutes to obtain solution S2. The amount of the isocyanate compound added is determined according to the amount of hydroxyl groups on the polyethylene glycol, and the ratio of the N=C=O mole number of the isocyanate compound to the hydroxyl mole number of the polyethylene glycol is generally 1 to 2.

[0071] Step 3: Place the solution S2 obtained in step 2 in an oil bath at 50° C. and stir at a constant temperature of 200 rpm for 4 hours to obtain a reaction solution S3.

[0072] Step 4: After the reaction solution S3 obtained in step 3 is cooled to room temperature, 0.27 g of hexamethylenediamine is added and stirring is continued for 20 min to obtain reaction solution S4. The reaction solution S4 is then poured into a culture dish and allowed to stand in a fume hood at room temperature for 12 h. The mixture is then dried in a vacuum oven at 55° C. for 3 h to obtain a modified polyethylene glycol material.

[0073] Performance test of Example 3:

[0074] In this embodiment, the gas volume method was used to test to evaluate the interaction and chemical compatibility between the modified polyethylene glycol material and ammonium dinitramide. It should be noted that in this embodiment, the test results of ammonium dinitramide were taken from the test results in Example 1. The specific process of the test is as follows:

[0075] First, 0.5 g of the modified polyethylene glycol material after drying and removing the solvent and 0.5 g of ammonium dinitramide were weighed, mixed and placed in the first reaction tank; 0.5 g of unmodified polyethylene glycol and 0.5 g of ammonium dinitramide were weighed, mixed and placed in the second reaction tank; 1.0 g of the modified polyethylene glycol material after drying and removing the solvent was weighed and placed in the third reaction tank.

[0076] Then assemble the three reaction cells into the reaction tube, connect the pressure sensor and the reaction tube with a pressure line, and tighten to ensure airtightness; then place the reaction tube in a stable 100°C constant temperature furnace, start heating, and record the pressure-time data at the same time. After heating for 40 hours, take out the reaction tube, and qualitatively judge the degree of interaction by the pressure change, and quantitatively judge the compatibility by the amount of outgassing.

[0077] In this embodiment, the test results and evaluations are as follows:

[0078] The measured data were converted into the gas release under standard conditions, and the results were as follows: the gas release of the modified polyethylene glycol material was 0 mL, the gas release of ammonium dinitramide was 0.65 mL, the gas release of the unmodified polyethylene glycol and ammonium dinitramide was 9.03 mL, and the gas release of the modified polyethylene glycol material and ammonium dinitramide was 0.23 mL. From the gas release results, it can be seen that the interaction between the modified polyethylene glycol material and ammonium dinitramide is weak, and the chemical compatibility of the modified polyethylene glycol material and ammonium dinitramide is much better than that of the unmodified polyethylene glycol and ammonium dinitramide.

[0079] Embodiment 4:

[0080] This embodiment provides a method for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds, which uses modified hydroxyl-containing polymer materials to improve the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds. The method for modifying hydroxyl-containing polymer compounds includes the following steps:

[0081] Step 1, weigh 3g of polyethylene glycol, add 60g of ethyl acetate, stir with a glass rod during the addition, so that the polyethylene glycol and ethyl acetate are fully in contact, accelerate the dissolution of the polyethylene glycol, and shorten the dissolution time; then place it on an oscillating screen and oscillate for 1h. After the oscillation is completed, let it stand at room temperature for 12h. After the polyethylene glycol is dissolved, a polyethylene glycol solution S1 is obtained.

[0082] Step 2: Add 0.72 g of isopropyl isocyanate to the polyethylene glycol solution S1 obtained in step 1, and then add 6 mg of dibutyltin dilaurate, and stir at 200 rpm for 30 minutes to obtain solution S2.

[0083] Step 3: Place the solution S2 obtained in step 2 in an oil bath at 50° C. and stir at a constant temperature of 200 rpm for 4 hours to obtain a reaction solution S3.

[0084] Step 4: Pour the reaction solution S3 obtained in step 3 into a culture dish, let it stand in a fume hood at room temperature for 12 hours, and then dry it in a vacuum oven at 55° C. for 3 hours to obtain a modified polyethylene glycol material.

[0085] Performance test of embodiment 4:

[0086] In this embodiment, the gas volume method was used to test the interaction and chemical compatibility between the modified polyethylene glycol material and ammonium dinitramide. It should be noted that in this embodiment, the test results of ammonium dinitramide are the test results in Example 1; the test results of unmodified polyethylene glycol and ammonium dinitramide are the test results in Example 3. The specific process of the test is as follows:

[0087] First, 0.5 g of the modified polyethylene glycol material after drying and removing the solvent and 0.5 g of ammonium dinitramide were weighed, mixed and placed in the first reaction tank; 1.0 g of the modified polyethylene glycol material after drying and removing the solvent was weighed and placed in the second reaction tank.

[0088] Then assemble the two reaction cells into the reaction tube, connect the pressure sensor and the reaction tube with a pressure line, and tighten to ensure airtightness; then place the reaction tube in a stable 100°C constant temperature furnace, start heating, and record the pressure-time data at the same time. After heating for 40 hours, take out the reaction tube, and qualitatively judge the degree of interaction by the pressure change, and quantitatively judge the compatibility by the amount of outgassing.

[0089] In this embodiment, the test results and evaluations are as follows:

[0090] like Figure 3 As shown, the pressure of the modified polyethylene glycol material and ammonium dinitramide is much lower than that of polyethylene glycol and ammonium dinitramide, indicating that the interaction between the modified polyethylene glycol material and ammonium dinitramide is weak and the compatibility is good. The measured data were converted into the degassing volume under standard conditions, and the results were as follows: the degassing volume of the modified polyethylene glycol material was 0.06mL, the degassing volume of ammonium dinitramide was 0.65mL, the degassing volume of the unmodified polyethylene glycol and ammonium dinitramide was 9.03mL, and the degassing volume of the modified polyethylene glycol material and ammonium dinitramide was 0.56mL. From the degassing volume results, it can be seen that the chemical compatibility of the modified polyethylene glycol material and ammonium dinitramide is much better than that of the unmodified polyethylene glycol and ammonium dinitramide.

Claims

1. A method for improving the compatibility of ammonium dinitramide and a hydroxyl-containing polymer compound, characterized in that: The method uses a monoisocyanate compound to modify a hydroxyl-containing polymer compound to improve the compatibility of ammonium dinitramide and the hydroxyl-containing polymer compound; the method specifically comprises the following steps: Step 1, adding a solvent to a hydroxyl-containing polymer compound, stirring while adding, shaking after adding, standing after shaking, and preparing a solution S1 after the hydroxyl-containing polymer compound is dissolved; the hydroxyl-containing polymer compound is nitrocellulose or polyethylene glycol; the solvent is ethyl acetate; Step 2, adding a monoisocyanate compound to the solution S1 obtained in step 1, and then adding a catalyst, and stirring to obtain a solution S2; the monoisocyanate compound is propyl isocyanate, hexyl isocyanate or octyl isocyanate; Step 3, heating and stirring the solution S2 obtained in step 2 to obtain a reaction solution S3; the heating and stirring conditions are: stirring at a constant temperature of 100 rpm to 500 rpm for 4 h to 12 h in an oil bath at 25° C. to 80° C.; Step 4: The reaction solution S3 obtained in step 3 is allowed to stand and dry to obtain a modified hydroxyl-containing polymer material.

2. The method for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds as claimed in claim 1, characterized in that: The catalyst is dibutyltin dilaurate or stannous octoate.

3. The method for improving the compatibility of ammonium dinitramide and hydroxyl-containing polymer compounds as claimed in claim 1, characterized in that: In step 2, the stirring condition is: stirring at a speed of 100 rpm to 500 rpm for 0.5 h to 48 h.