Carbon negative electrode and preparation method thereof, lithium ion battery

By using N-doped carbon materials with a hollow spherical structure and MoC nanoparticles embedded in the carbon anode material, the problem of insufficient thermodynamic stability of the carbon anode material in lithium-ion batteries is solved, and the energy density and cycle stability of the battery are improved.

CN115939327BActive Publication Date: 2024-10-01CHONGQING TALENT NEW ENERGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211689772.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-10-01
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

Existing carbon anode materials have poor thermodynamic stability in lithium-ion batteries, which affects ion transmission and the deintercalation of lithium ions, resulting in the need to improve the energy density and cycle stability of the battery.

Method used

A carbon material layer with a hollow sphere structure is used, and MoC nanoparticles are embedded in the shell. Through the preparation method of Mo-based ZIF series metal organic framework materials, tannic acid etching and pyrolysis are used to form N-doped carbon materials to enhance the material's Thermodynamic stability and spatial structure.

Benefits of technology

It improves the transmission efficiency and intercalation and deintercalation capabilities of lithium ions, suppresses the volume expansion of active materials, and significantly improves the energy density and cycle stability of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115939327B_ABST
    Figure CN115939327B_ABST
Patent Text Reader

Abstract

The present application discloses a carbon negative electrode and a preparation method thereof, and a lithium ion battery, wherein the carbon negative electrode comprises a negative electrode current collector and a carbon material located on the surface of the negative electrode current collector, the carbon material is a hollow spherical structure, and the shell of the hollow spherical structure comprises an N-doped carbon matrix embedded with MoC nanoparticles. The hollow structure of the embodiment of the present application is conducive to the transmission of lithium ions and ion embedding and de-embedding, and the N-doped carbon material derived from MOFs can increase the thermodynamic stability of the carbon material, and has a larger spatial structure, which is conducive to suppressing the volume expansion of the active material, thereby improving the energy density and stability of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to the field of new energy, and specifically relates to a carbon negative electrode and a preparation method thereof, and a lithium ion battery. Background Art

[0002] Lithium-ion batteries have better performance in terms of energy density and service life, so lithium-ion batteries have become a research hotspot in recent years. Carbon materials, as electrode materials for lithium-ion batteries, can achieve rapid insertion and extraction of lithium ions during the charging and discharging process, and show broad prospects in high-energy and high-power energy storage applications. However, existing carbon negative electrode materials still have poor thermodynamic stability, which affects ion transport and lithium ion extraction, resulting in the battery's energy density and cycle stability needing to be further improved. Summary of the invention

[0003] In view of the above-mentioned defects or deficiencies in the prior art, it is desired to provide a carbon negative electrode and a preparation method thereof, and a lithium ion battery.

[0004] In a first aspect, the present invention provides a carbon negative electrode, comprising a negative electrode current collector and a carbon material layer located on the surface of the negative electrode current collector, wherein the carbon material layer is a hollow spherical structure, and the shell layer of the hollow spherical structure comprises an N-doped carbon matrix in which MoC nanoparticles are embedded.

[0005] As a preferred solution, the thickness of the carbon material layer is 50um-100um.

[0006] As a preferred solution, the shell layer of the hollow spherical structure further includes cobalt particles or nickel particles.

[0007] As a preferred solution, the inner diameter of the hollow sphere is 1um-2um.

[0008] In a second aspect, the present application provides a method for preparing the carbon negative electrode of the first aspect, comprising the following steps:

[0009] Preparation of carbon materials:

[0010] The Mo-based ZIF series metal organic framework material is dispersed in a solution of tannic acid and water, stirred at room temperature for reaction, and then washed and dried to obtain a hollow Mo-based ZIF series metal organic framework material;

[0011] The hollow Mo-based ZIF series metal-organic framework material is pyrolyzed in an inert atmosphere and naturally cooled to room temperature to obtain a carbon material;

[0012] Preparation of carbon negative electrode:

[0013] The carbon material, the conductive agent and the adhesive are mixed in proportion, fully ground and dripped with a solvent, and ground evenly to obtain a negative electrode slurry;

[0014] The negative electrode slurry is coated on the negative electrode current collector, dried, and then subjected to cold pressing and slitting processes to obtain a carbon negative electrode.

[0015] As a preferred solution, the preparation method of Mo-based ZIF series metal organic framework materials is as follows: a mixture of metal salt, 2-methylimidazole, H2MoO4 and solvent is stirred and refluxed to fully react, and then naturally cooled, filtered, washed, and dried to obtain Mo-based ZIF series metal organic framework materials.

[0016] As a preferred solution, the mass ratio of Mo-based ZIF series metal organic framework materials, tannic acid and water is (0.06-0.2):1:(50-200).

[0017] As a preferred solution, the metal salt is selected from at least one of zinc salt, cobalt salt and nickel salt;

[0018] Preferably, the zinc salt is selected from any one of zinc acetate, zinc chloride, zinc nitrate and zinc sulfate;

[0019] The cobalt salt is selected from at least one of cobalt nitrate and cobalt acetate;

[0020] The nickel salt is selected from at least one of nickel nitrate, nickel sulfate and nickel chloride.

[0021] As a preferred solution, the mass ratio of Mo-based ZIF series metal organic framework materials, tannic acid and water is (0.1-0.15):1:(100-200).

[0022] As a preferred solution, in the process of dispersing the Mo-based ZIF series metal-organic framework material in a solution of tannic acid and water, stirring the reaction at room temperature, washing and drying to obtain the hollow Mo-based ZIF series metal-organic framework material, the stirring reaction time is 10 min-30 min.

[0023] As a preferred solution, in the process of pyrolyzing the hollow Mo-based ZIF series metal organic framework material under an inert atmosphere and naturally cooling it to room temperature to obtain the carbon material, the pyrolysis temperature is 700°C-900°C.

[0024] In a third aspect, the present invention provides a lithium-ion battery comprising the carbon negative electrode of the first aspect.

[0025] The carbon negative electrode provided by the present invention has a hollow spherical structure in which the carbon material is conducive to the transmission, embedding and de-embedding of lithium ions, and the N-doped carbon material derived from MOFs can increase the thermodynamic stability of the carbon material and has a large spatial structure, which is conducive to suppressing the volume expansion of the active material, thereby improving the energy density and stability of the lithium-ion battery; and, the present invention pyrolyzes the precursor of the synthesized ZnMo bimetallic organic crystalline framework, volatilizes the metal Zn element nodes during the pyrolysis process, increases the pore volume after pyrolysis, and maintains the hollow sphere morphology unchanged, thereby forming a structure in which MoC nanoparticles are embedded in the carbon layer, and the preparation method is simple and controllable. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments made with reference to the following drawings:

[0027] Figure 1 This is a scanning electron microscope photograph (8 um) of a carbon material on a carbon negative electrode of Example 1 of the present invention;

[0028] Figure 2 This is a scanning electron microscope photograph (1 um) of a carbon material on a carbon negative electrode of Example 1 of the present invention;

[0029] Figure 3 The battery cycle performance test results of Examples 1-6 and Comparative Examples 1-2 of the present invention are shown;

[0030] Figure 4 The battery cycle performance test results of Example 1 and Examples 6-7 of the present invention are as follows;

[0031] Figure 5 The battery cycle performance test results of Examples 1 and 8-10 of the present invention are shown. DETAILED DESCRIPTION

[0032] The present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention.

[0033] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail with reference to the embodiments below.

[0034] In a first aspect, an embodiment of the present invention provides a carbon negative electrode, including a negative electrode current collector and a carbon material layer located on the surface of the negative electrode current collector, such as Figure 1 and Figure 2 As shown, the carbon material layer is a hollow spherical structure, and the shell layer of the hollow spherical structure includes an N-doped carbon matrix in which MoC nanoparticles are embedded.

[0035] It can be understood that the carbon material layer serves as the active material of the negative electrode, and the hollow spherical structure has a high specific surface area and porosity, which is beneficial to lithium ion transmission and lithium ion embedding and de-embedding; the shell layer of the hollow spherical structure includes an N-doped carbon matrix embedded with MoC nanoparticles, forming a rich nanoscale MoC / NC heterogeneous interface. MoC has a hexagonal crystal structure and partially overlaps atomic orbitals to construct a special charge channel, which is beneficial to the smooth migration and uniform deposition of lithium ions. The heterogeneous interface is beneficial to accelerate the diffusion of lithium ions and improve the ion transmission efficiency. Nitrogen-doped carbon increases the thermodynamic stability of the carbon material, and the hollow spherical structure has a larger spatial structure, which is beneficial to inhibit the volume expansion of the active material, thereby improving the energy density and cycle stability of the battery.

[0036] In some embodiments, the thickness of the carbon material layer is 50um-100um, which can ensure the ion transmission of the material and the embedding and de-embedding of ions. The thickness of the carbon material refers to the thickness of the carbon material coated on the surface of the negative electrode current collector, which can be any value in this interval, such as 50um, 60um, 70um, 80um, 90um or 100um. If the coating thickness of the carbon material layer is too thick, the lithium ion transmission efficiency is low, and if it is too thin, the activity is low, resulting in a decrease in battery performance.

[0037] In some embodiments, the shell layer of the hollow spherical structure further includes cobalt particles or nickel particles.

[0038] Furthermore, the inner diameter of the hollow sphere is 1um-2um. Among them, the inner diameter of the hollow sphere refers to the diameter of the hollow sphere minus twice the wall thickness of the hollow sphere. The inner diameter range disclosed in this embodiment can better allow lithium ions to enter the interior of the negative electrode material to increase the load and transmission capacity of lithium ions; if it is larger than this range, the hollow structure will be damaged because the diameter of the MOFs sphere is about 2um. If it is less than 1um, it means that the etching is insufficient, resulting in the inability of ions to smoothly enter the interior of the negative electrode material, and also reducing the transportation and load capacity of lithium ions.

[0039] In a second aspect, the present application provides a method for preparing the carbon negative electrode of the first aspect, comprising the following steps:

[0040] Preparation of carbon materials:

[0041] S1, dispersing a Mo-based ZIF series metal organic framework material in a solution of tannic acid and water, stirring at room temperature for reaction, washing and drying to obtain a hollow Mo-based ZIF series metal organic framework material;

[0042] It should be noted that the Mo-based ZIF series metal organic framework material is dispersed in a solution of tannic acid and water, the purpose of which is to use tannic acid to etch the Mo-based ZIF series metal organic framework material. The morphology of the Mo-based ZIF series metal organic framework material before etching is a regular polyhedron, and tannic acid can destroy the coordination between metals. After etching, the Mo-based ZIF series metal organic framework material forms a hollow spherical structure. Among them, the stirring can be magnetic stirring or mechanical stirring; the drying method can be air drying, vacuum drying or freeze drying, which is not limited in the embodiments of the present application.

[0043] In one embodiment of the present application, the mass ratio of the Mo-based ZIF series metal-organic framework material, the tannic acid and the water is (0.06-0.2):1:(50-200). The mass ratio of the three is within this range, which is conducive to ensuring that the Mo-based ZIF series metal-organic framework material is completely etched to form a spherical structure, avoiding too little tannic acid, which cannot fully etch the Mo-based ZIF series metal-organic framework material, or too much tannic acid, which causes the Mo-based ZIF series metal-organic framework material to collapse after etching and cannot form a spherical structure.

[0044] S3, placing the hollow Mo-based ZIF series metal organic framework material in an inert atmosphere for high temperature pyrolysis, and naturally cooling to room temperature to obtain a carbon material;

[0045] Among them, the inert atmosphere can be nitrogen or argon, etc., which is beneficial to protect the hollow Mo-based ZIF series metal-organic framework materials from reacting with air during high-temperature pyrolysis, reduce the occurrence of side reactions, and thus ensure the structure of the material.

[0046] During the high-temperature pyrolysis process in the embodiment of the present application, the inner diameter of the hollow spherical structure increases, the morphology of the hollow sphere remains unchanged, and the material is further carbonized, thereby forming a hollow spherical structure in which MoC nanoparticles are embedded in the carbon shell layer.

[0047] Preparation of carbon negative electrode:

[0048] S4, mixing the carbon material, the conductive agent and the adhesive according to a proportion, grinding them fully and adding a solvent dropwise, grinding them evenly to obtain a negative electrode slurry;

[0049] S5. The negative electrode slurry is coated on the negative electrode current collector, dried, and then subjected to cold pressing and slitting processes to obtain a carbon negative electrode.

[0050] In summary, the carbon negative electrode preparation process of the embodiment of the present application is simple and controllable, the hollow structure of the prepared carbon negative electrode material is conducive to the transmission of lithium ions and the insertion and deinsertion of lithium ions, and the N-doped carbon material derived from MOFs can increase the thermodynamic stability of the carbon material and has a larger spatial structure, which is conducive to inhibiting the volume expansion of the active material, thereby improving the energy density and stability of the lithium-ion battery.

[0051] In some embodiments, S1, stirring and refluxing a mixture of a metal salt, 2-methylimidazole, H2MoO4 and a solvent to fully react, naturally cooling, filtering, washing, and drying to obtain a Mo-based ZIF series metal organic framework material;

[0052] It can be understood that in step S1, the precursor of the bimetallic organic framework is prepared, wherein the metal salt can be any one except Mo salt, such as zinc salt, cobalt salt or nickel salt, and specifically can be zinc acetate, cobalt nitrate, cobalt acetate, nickel nitrate, etc., which is not specifically limited in the embodiment of the present application;

[0053] It should be noted that when zinc salt is selected, the metal nodes of the prepared bimetallic organic framework precursor will decompose and volatilize after the subsequent pyrolysis treatment, and there will be no metal ions on the surface of the MOFs (metal organic framework) material; when nickel salt, cobalt salt or other metal salt is selected, the metal nodes will not volatilize during the heat treatment process, and metal ions will increase on the surface of the MOFs material. For example, when cobalt nitrate is used, Co / MoC / NC will be formed on the surface of the hollow MOFs after pyrolysis; the cobalt element or other metal elements in the carbon material shell can stabilize the structure of the material and improve the cycle performance and rate performance of the material, but excessive other metal elements will also lead to a decrease in the actual capacity of the battery.

[0054] For example, in actual preparation, a mixture of metal salt, 2-methylimidazole, H2MoO4 and 120 mL of DMF was placed in a 250 mL round-bottom flask, stirred and reacted at 160°C for 6 hours, naturally cooled to room temperature, filtered and washed three times with ethanol, and dried at room temperature to obtain Mo-based ZIF series metal organic framework materials.

[0055] Furthermore, in the process of stirring a mixture of metal salt, 2-methylimidazole, H2MoO4 and DMF to fully react, naturally cooling, filtering, washing, and drying to obtain a Mo-based ZIF series metal organic framework material, the metal salt is selected from zinc salts, and preferably, the zinc salt is selected from any one of zinc acetate, zinc chloride, zinc nitrate and zinc sulfate.

[0056] In this embodiment, zinc salt is selected to prepare a hollow Mo-based ZIF series metal-organic framework material, which is a ZnMo-bimetallic organic framework. During high-temperature pyrolysis, the Zn element node is easily volatile, so that the metal element on the surface of the final carbon material is single, and no other metal elements are introduced. When used as a negative electrode material, it is beneficial to improve the embedding and de-embedding of lithium ions, thereby improving the battery performance of lithium ions.

[0057] In a preferred embodiment, in the process of dispersing the Mo-based ZIF series metal-organic framework material in a solution of tannic acid and water, stirring the reaction at room temperature, washing and drying to obtain a hollow Mo-based ZIF series metal-organic framework material, the mass ratio of the Mo-based ZIF series metal-organic framework material, tannic acid and water is (0.1-0.15):1:(100-200).

[0058] It can be understood that the mass ratio of the Mo-based ZIF series metal-organic framework material, tannic acid and water is 0.1:1:100, 0.12:1:150, 0.15:1:200, etc. The value range of the mass ratio of the Mo-based ZIF series metal-organic framework material, tannic acid and water disclosed in this embodiment is conducive to ensuring that the Mo-based ZIF series metal-organic framework material is completely etched to form a hollow spherical structure.

[0059] Furthermore, in the process of dispersing the Mo-based ZIF series metal-organic framework material in a solution of tannic acid and water, stirring the reaction at room temperature, washing and drying to obtain the hollow Mo-based ZIF series metal-organic framework material, the stirring reaction time is 10 min-30 min.

[0060] Among them, the stirring reaction time can be understood as the etching time, and the stirring reaction time can be 10min, 15min, 20min, 25min or 30min. The stirring time disclosed in the embodiment of the present application is conducive to the complete etching of the hollow Mo-based ZIF series metal organic framework material, and ensures the morphology structure of the powder, avoids excessive etching to destroy the morphology structure, and is also conducive to saving processing time and improving preparation efficiency.

[0061] Further, when the Mo-based ZIF series metal-organic framework material is dispersed in a solution of tannic acid and water, the reaction is stirred at room temperature, and then washed and dried to obtain a hollow Mo-based ZIF series metal-organic framework material, the washing method is to wash with water and ethanol 2-3 times respectively. It is understandable that in the actual preparation process, ethanol can be used for washing 2-3 times, and then water can be used for washing 2-3 times; of course, water can be used for washing 2-3 times, and then ethanol can be used for washing 2-3 times. It can be adjusted according to the actual situation, and the embodiment of the present application does not specifically limit this. The washing method of the embodiment of the present application uses ethanol to thoroughly clean the residual organic solvent, and then washes with water to ensure that other residual substances are washed away, reducing impurities in the hollow Mo-based ZIF series metal-organic framework material, which is conducive to ensuring the purity of subsequent carbon materials.

[0062] In a preferred embodiment, in the process of dispersing the Mo-based ZIF series metal-organic framework material in a solution of tannic acid and water, stirring the reaction at room temperature, washing and drying to obtain a hollow Mo-based ZIF series metal-organic framework material, the drying method is vacuum drying, the drying temperature is 40-60°C, and the drying time is 2h-5h.

[0063] The embodiment of the present application adopts a vacuum drying method, and the drying conditions are mild, which is conducive to ensuring the morphology and structure of the hollow Mo-based ZIF series metal organic framework materials, while avoiding side reactions between the material and the air during the drying process.

[0064] Furthermore, in the process of pyrolyzing the hollow Mo-based ZIF series metal organic framework material under an inert atmosphere and naturally cooling it to room temperature to obtain the carbon material, the pyrolysis temperature is 700°C-900°C.

[0065] The embodiment of the present application adopts a programmed temperature rising technology to raise the temperature from room temperature to the pyrolysis temperature at a certain heating rate, and maintains the temperature for a certain time, so that the hollow Mo-based ZIF series metal organic framework material undergoes a pyrolysis reaction to form a spherical structure in which MoC is embedded in the nitrogen-doped carbon layer. In a specific embodiment, the heating rate can be 5°C / min-8°C / min, and the pyrolysis time can be 2h-4h.

[0066] The heating rate disclosed in the embodiment of the present application is conducive to ensuring the decomposition of metal elements in the material during the heating stage, avoiding the heating rate being too fast and the decomposition reaction being incomplete, and at the same time avoiding the heating rate being too low and the material being highly carbonized, and the metal elements being coated and unable to decompose; the pyrolysis temperature is easy to achieve, and the processing is safe and reliable, which is conducive to ensuring better carbonization of the material and forming a spherical structure of MoC embedded in a nitrogen-doped carbon layer, avoiding the temperature being too low to achieve the ideal carbonization degree, and the temperature being too high to cause the spherical structure of the material to collapse; the pyrolysis time ensures the full carbonization of the material and the growth of the morphology, while saving preparation time.

[0067] In summary, the preparation method of the carbon negative electrode of the embodiment of the present application is simple and controllable to operate. Through the process of tannic acid etching and pyrolysis, a carbon material with a hollow spherical structure is constructed, which is conducive to the transmission of ions and the insertion and deinsertion of ions. The N-doped carbon material derived from MOFs can increase the thermodynamic stability and has a larger spatial structure, which can reduce the volume expansion of the active material, thereby greatly improving the energy density and stability.

[0068] In a third aspect, the present invention provides a lithium ion battery, comprising the carbon negative electrode of the first aspect. Thus, the lithium ion battery has all the characteristics and advantages of the carbon negative electrode described above, which will not be described in detail here.

[0069] In a specific embodiment, the preparation method of the lithium ion battery is as follows:

[0070] Step 1, placing a mixture of Zn(CH3COO)2·2H2O, 2-methylimidazole (2-mim), H2MoO4 and 120mL DMF in a 250ml round-bottom flask, stirring and refluxing at 160°C for 6 hours, cooling naturally, filtering and washing three times with ethanol, and drying at room temperature to obtain a white Mo-based ZIF series metal organic framework material;

[0071] Step 2, dispersing 0.3 g of Mo-based ZIF series metal organic framework material in a solution of 1.5 g of tannic acid and 300 mL of water, stirring at room temperature for 10 min, washing by centrifugation with water and ethanol for 3 times, and drying in a vacuum oven at 60° C. for 3 hours to obtain a hollow Mo-based ZIF series metal organic framework material;

[0072] Step 3, placing the hollow Mo-based ZIF series metal organic framework material into a corundum boat, raising the temperature to 700°C at 8°C / min in a nitrogen atmosphere, keeping the temperature constant for 2 hours, and then naturally cooling to room temperature to obtain a carbon material;

[0073] Step 4, mixing the carbon material, carbon black and polyvinylidene fluoride in a ratio of 8:1:1, grinding them thoroughly, adding N-methylpyrrolidone dropwise, and continuing grinding to form a uniform negative electrode slurry;

[0074] Step 5, subjecting a copper foil of a certain thickness to ultrasonic treatment in an ethanol solution, and then placing the copper foil in a forced air drying oven for drying;

[0075] Step 6, use a scraper to scrape 100 microns of the negative electrode slurry obtained in step 4 onto the above copper foil, then place it in an 80°C forced air drying oven for drying, use a sheet press to make a circular electrode sheet with a diameter of 14 mm, place it in a vacuum drying oven at 60°C for drying, and make a negative electrode sheet.

[0076] Step 7, assemble the negative electrode sheet and the positive lithium sheet into a button battery in a glove box filled with argon Ar in the order of positive electrode shell, negative electrode sheet, electrolyte, diaphragm, lithium sheet, gasket, spring and negative electrode shell.

[0077] It is also understandable that the lithium-ion battery can also be applied to electric vehicles or any energy storage device. Therefore, the energy storage device or electric vehicle has all the features and advantages of the above-mentioned diaphragm, which will not be repeated here.

[0078] The present invention is described below by means of specific examples. It should be noted that the following specific examples are only for illustrative purposes and do not limit the scope of the present invention in any way. In addition, unless otherwise specified, methods without specific conditions or steps are conventional methods, and the reagents and materials used can be obtained from commercial channels.

[0079] Example 1

[0080] A mixture of 5.28 g Zn(CH3COO)2·2H2O, 2.88 g 2-methylimidazole (2-mim), 0.99 g H2MoO4 and 120 mL DMF was placed in a 250 ml round-bottom flask, stirred at 160 °C for 6 hours, cooled naturally, filtered and washed three times with ethanol, and dried at room temperature to obtain a white Mo-based ZIF series metal-organic framework material;

[0081] 0.2 g of Mo-based ZIF series metal-organic framework material was dispersed in a solution of 1 g of tannic acid and 200 mL of water, stirred at room temperature for 10 min, washed by centrifugation with water and ethanol for 3 times, and dried in a vacuum oven at 60 ° C for 3 hours to obtain a hollow Mo-based ZIF series metal-organic framework material;

[0082] The hollow Mo-based ZIF series metal organic framework material was placed in a corundum boat, and the temperature was raised to a pyrolysis temperature of 900°C at 8°C / min in a nitrogen atmosphere, and then the temperature was kept constant for 2 hours, and then the temperature was naturally cooled to room temperature to obtain a carbon material.

[0083] The carbon material, carbon black and polyvinylidene fluoride are mixed in a mass ratio of 8:1:1, fully ground and 4-7 drops of N-methylpyrrolidone are added, and the grinding is continued to form a uniform negative electrode slurry;

[0084] The negative electrode slurry is coated on a copper foil, and after the copper foil is dried, it is subjected to cold pressing and slitting processes to obtain a carbon negative electrode, wherein the thickness of the carbon material layer is 60 microns;

[0085] The carbon negative electrode and the positive lithium sheet were assembled into a button battery in a glove box filled with argon Ar in the order of positive electrode shell, negative electrode sheet, 200-300 μl lithium hexafluorophosphate electrolyte, commercial 2400 separator, lithium sheet, gasket, shrapnel and negative electrode shell.

[0086] Example 2

[0087] Different from the above-mentioned Example 1, in this example, the mass ratio of the Mo-based ZIF series metal organic framework material, tannic acid and water is 0.06:1:50.

[0088] Example 3

[0089] Different from the above-mentioned Example 1, in this example, the mass ratio of the Mo-based ZIF series metal organic framework material, tannic acid and water is 0.1:1:125.

[0090] Example 4

[0091] Different from the above-mentioned Example 1, in this example, the mass ratio of the Mo-based ZIF series metal organic framework material, tannic acid and water is 0.15:1:150.

[0092] Example 5

[0093] Different from the above-mentioned Example 1, in this example, the mass ratio of the Mo-based ZIF series metal organic framework material, tannic acid and water is 0.12:1:100.

[0094] Example 6

[0095] Different from the above-mentioned Example 1, in this example, 0.2 g of Mo-based ZIF series metal organic framework material is dispersed in a solution of 1 g of tannic acid and 200 mL of water, and stirred at room temperature for 20 min.

[0096] Example 7

[0097] Different from the above-mentioned Example 1, in this example, 0.2 g of Mo-based ZIF series metal organic framework material was dispersed in a solution of 1 g of tannic acid and 200 mL of water, and stirred at room temperature for 30 min.

[0098] Example 8

[0099] Different from the above-mentioned embodiment 1, in the process of preparing the hollow Mo-based ZIF series metal organic framework material into the carbon material, the pyrolysis temperature is 700°C.

[0100] Example 9

[0101] Different from the above-mentioned embodiment 1, in the process of preparing the hollow Mo-based ZIF series metal organic framework material into the carbon material, the pyrolysis temperature is 500°C.

[0102] Example 10

[0103] Different from the above-mentioned embodiment 1, in the process of preparing the hollow Mo-based ZIF series metal organic framework material into the carbon material, the pyrolysis temperature is 1200°C.

[0104] Comparative Example 1

[0105] Different from the above-mentioned Example 1, in this comparative example, the mass ratio of the Mo-based ZIF series metal organic framework material, the tannic acid and the water is 0.01:1:200.

[0106] Comparative Example 2

[0107] Different from the above-mentioned Example 1, in this comparative example, the mass ratio of the Mo-based ZIF series metal organic framework material, the tannic acid and the water is 1:1:200.

[0108] The carbon materials prepared in Examples 1 to 10 were subjected to SEM testing, and typically as shown in Example 1, Figure 1 and Figure 2 The SEM images of the carbon material prepared in Example 1 at different magnifications show that Figure 1 It can be seen that the carbon material is a spherical structure. Figure 2 It can be clearly seen that the interior of the carbon material sphere is a hollow structure, and the inner diameter of the hollow sphere is 1.7um.

[0109] The following describes the performance test process and test results of lithium-ion batteries:

[0110] (1) Gram capacity

[0111] The first discharge capacity / mass of active material, where the mass of the negative electrode active material is 4 mg.

[0112] (2) Cycle test

[0113] After the battery is charged to 3V at a constant current of 0.2C, it is charged at a constant voltage until the cut-off current is 0.2C, left to stand for 5 minutes, and then discharged to 1.5V at a constant current of 0.2C. This is recorded as one charge and discharge cycle. 50 cycles are performed under the above conditions; the capacity retention rate (%) of the battery after 50 cycles / 3.0V cycles = (discharge capacity of the 50th cycle / discharge capacity of the first cycle) × 100%;

[0114] The results of the lithium ion batteries of Examples 1-10 and Comparative Examples 1-2 tested according to the above process and method are shown in Table 1:

[0115] Table 1 Test results of Examples 1-10 and Comparative Examples 1-2

[0116]

[0117] It can be seen from Table 1 that Examples 1-8 have a higher gram capacity, that is, a high energy density, which proves that the hollow sphere structure of the present invention can effectively inhibit the volume expansion of the active material, thereby improving the energy density of the lithium-ion battery. Examples 9 and 10 have a decrease in gram capacity due to the pyrolysis temperature being too high or too low.

[0118] from Figure 3It can be seen that the battery test results of Examples 1-6 are significantly better than those of Comparative Examples 1 and 2, indicating that the mass ratio range of the Mo-based ZIF series metal-organic framework material, tannic acid and water disclosed in the embodiments of the present application is conducive to ensuring that the Mo-based ZIF series metal-organic framework material is completely etched to form a spherical structure, which is beneficial to the transmission of ions and the insertion and deinsertion of ions. The N-doped carbon material derived from MOFs can increase the thermodynamic stability and has a larger spatial structure, which can reduce the volume expansion of the active material, thereby improving the gram capacity and cycle stability of the battery; excessive ZIF series metal-organic framework material leads to incomplete etching and the inability to form a hollow spherical structure. Excessive tannic acid leads to excessive etching, destroys the material structure, and causes a decrease in battery performance.

[0119] from Figure 4 It can be seen that the battery test results of Example 1 and Examples 6-7 indicate that the stirring time disclosed in the examples of the present application can ensure the hollow spherical structure of the material, so that the battery has a higher gram capacity and good cycle stability.

[0120] from Figure 5 It can be seen that the battery test results of Examples 1 and 8 are significantly better than those of Examples 9 and 10, indicating that the pyrolysis temperature disclosed in the examples of the present application is conducive to ensuring the carbonization degree of the material and forming a spherical structure of MoC embedded in the nitrogen-doped carbon layer, thereby improving the gram capacity and cycle stability of the battery.

[0121] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.

Claims

1. A method for preparing a carbon negative electrode, characterized in that: The steps include: Preparation of carbon materials: The Mo-based ZIF series metal organic framework material is dispersed in a solution of tannic acid and water, and after stirring at room temperature for reaction, the hollow Mo-based ZIF series metal organic framework material is obtained by washing and drying, wherein the mass ratio of the Mo-based ZIF series metal organic framework material, the tannic acid and the water is (0.1-0.15):1:(100-200); The hollow Mo-based ZIF series metal organic framework material is placed in an inert atmosphere for pyrolysis, and naturally cooled to room temperature to obtain the carbon material, wherein the carbon material is a hollow spherical structure, the shell layer of the hollow spherical structure includes MoC nanoparticles and an N-doped carbon matrix, the MoC nanoparticles are embedded in the N-doped carbon matrix, the shell layer of the hollow spherical structure also includes cobalt particles or nickel particles, and the inner diameter of the hollow sphere is 1um-2um; Preparation of carbon negative electrode: The carbon material, the conductive agent and the binder are mixed in proportion, fully ground and dripped with a solvent, and ground evenly to obtain a negative electrode slurry; The negative electrode slurry is coated on the negative electrode current collector, dried, and then subjected to cold pressing and slitting processes to obtain the carbon negative electrode.

2. The preparation method according to claim 1, characterized in that: The preparation method of the Mo-based ZIF series metal organic framework material is as follows: The mixture of metal salt, 2-methylimidazole, H2MoO4 and solvent is stirred and refluxed to fully react, and then naturally cooled, filtered, washed, and dried to obtain the Mo-based ZIF series metal organic framework material.

3. The preparation method according to claim 2, characterized in that: The metal salt is selected from at least one of zinc salt, cobalt salt and nickel salt.

4. The preparation method according to claim 3, characterized in that: The zinc salt is selected from any one of zinc acetate, zinc chloride, zinc nitrate and zinc sulfate; The cobalt salt is selected from at least one of cobalt nitrate and cobalt acetate; The nickel salt is selected from at least one of nickel nitrate, nickel sulfate and nickel chloride.

5. The preparation method according to claim 1, characterized in that: In the process of dispersing the Mo-based ZIF series metal organic framework material in a solution of tannic acid and water, stirring and reacting at room temperature, washing and drying to obtain a hollow Mo-based ZIF series metal organic framework material, the stirring reaction time is 10 min-30 min.

6. The preparation method according to claim 1, characterized in that: In the process of placing the hollow Mo-based ZIF series metal organic framework material under an inert atmosphere for pyrolysis and naturally cooling it to room temperature to obtain the carbon material, the pyrolysis temperature is 700°C-900°C.

7. The carbon negative electrode obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The carbon negative electrode comprises a negative electrode current collector and a carbon material layer located on the surface of the negative electrode current collector.

8. The carbon negative electrode according to claim 7, characterized in that The thickness of the carbon material layer is 50um-100um.

9. A lithium-ion battery, characterized in that Including the carbon negative electrode obtained by the preparation method according to any one of claims 1-6 or the carbon negative electrode according to any one of claims 7-8.

Citation Information

Patent Citations

  • Carbon-nitrogen compound hollow material and preparation method and application thereof

    CN106784687A

  • Nitrogen-doped porous hollow carbon sphere and preparation method and application thereof

    CN110729480A

  • Preparation of nitrogen-doped metal carbide material

    CN111244465A

  • Method for preparing battery negative electrode material by combining cavity precursor and ZIF derivative

    CN114094063A

  • Preparation method of Fe-doped Si / C composite material for negative electrode of lithium ion battery

    CN114883569A