Acridine fused ring substituted arylamine compound and application thereof

By using acridine fused ring-substituted aromatic amine compounds as hole transport materials for OLEDs, the problems of insufficient efficiency and lifetime of hole transport materials in the existing technology are solved, achieving higher luminous efficiency and longer service life, and simplifying process.

CN118724901APending Publication Date: 2024-10-01YANTAI XIANHUA CHEM TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310347820.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The hole transport material in existing OLEDs has a low hole migration rate and poor energy level matching, resulting in insufficient luminous efficiency and service life, which limits the development of display devices.

Method used

Acridine fused ring-substituted aromatic amine compounds are used as hole transport materials. Through their high bond energy and good solid-state stacking properties, the hole migration rate and luminous efficiency are improved, and the device life is extended.

Benefits of technology

It effectively reduces the driving voltage and improves the luminous efficiency and service life of OLED. At the same time, the process is simple and easy to implement, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724901A_ABST
    Figure CN118724901A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of organic light-emitting display, and particularly relates to an acridine fused ring substituted arylamine compound and application. The present invention provides a compound of formula (I) which can be used in hole transport materials. The compound has a parent structure of acridine fused ring substituted arylamine, has high bond energy between atoms and good thermal stability, is beneficial to solid-state accumulation between molecules, has strong hole transition ability, and can effectively reduce the voltage of a device and prolong the service life of the material when being used as a hole transport material. The invention also provides an organic electroluminescent device and a display device containing the compound shown in the formula (I). # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic light-emitting display, and in particular relates to an acridine condensed ring substituted aromatic amine compound and application thereof. Background Art

[0002] Electroluminescence (EL) refers to the phenomenon that luminescent materials emit light under the action of electric field and are stimulated by current and electric field. It is a luminescence process that directly converts electrical energy into light energy. Organic electroluminescent displays (hereinafter referred to as OLEDs) have a series of advantages such as autonomous luminescence, low-voltage DC drive, full curing, wide viewing angle, light weight, simple composition and process. Compared with liquid crystal displays, organic electroluminescent displays do not require backlight sources, have large viewing angles, low power consumption, and their response speed can reach 1000 times that of liquid crystal displays, but their manufacturing cost is lower than that of liquid crystal displays with the same resolution. Therefore, organic electroluminescent devices have a very broad application prospect.

[0003] Compared with inorganic luminescent materials, organic electroluminescent materials have many advantages, such as good processing performance, can be formed into films on any substrate by evaporation or spin coating, can realize flexible display and large-area display; can adjust the optical properties, electrical properties and stability of materials by changing the molecular structure, and there is a lot of room for material selection. In the most common OLED device structure, the following types of organic materials are usually included: hole injection materials, hole transport materials, electron transport materials, and various luminescent materials (dyes or doped guest materials) and corresponding host materials. Among them, hole transport materials, as an important functional material, have a direct impact on the mobility of holes and ultimately affect the luminous efficiency of OLEDs. However, the hole transport materials currently used in OLEDs can achieve a low hole migration rate, poor matching with the energy levels of adjacent layers, and cannot take into account both efficiency and life, which seriously restricts the display function and development of OLED display devices. Summary of the invention

[0004] The object of the present invention is to provide an acridine fused ring substituted aromatic amine compound and its application, which can be used as a hole transport material to improve the working efficiency and extend the service life of an organic electroluminescent device.

[0005] The first aspect of the present invention aims to provide an acridine fused ring substituted aromatic amine compound having a structure as shown in formula (I):

[0006]

[0007] in,

[0008] R 1 -R 2independently selected from C1-C3 alkyl, C3-C6 cycloalkane, C6-C 30 Aromatic groups;

[0009] R 3 -R 4 independently selected from C1-C3 alkyl, C3-C6 cycloalkane, C6-C 30 The aromatic group, and the adjacent substituents can be connected to form a ring;

[0010] Ar1-Ar4 are independently selected from C6-C 30 Aromatic or C3-C 30 heteroaryl;

[0011] m, n are selected from 0 or 1, and cannot be 0 at the same time;

[0012] The heteroatoms on the heteroaryl group are each independently selected from O, S or N;

[0013] The hydrogen atoms on the aromatic and heteroaryl groups may be independently substituted by Ra, wherein Ra is independently selected from deuterium, halogen, nitro, cyano, C1-C4 alkyl, C5-C 20 Cycloalkyl, phenyl, biphenyl, terphenyl or naphthyl.

[0014] Preferably, the R 1 -R 2 are independently selected from the following groups which are unsubstituted or substituted by Ra: methyl, ethyl, cyclopentyl, cyclohexyl, phenyl, biphenyl, naphthyl, phenanthrenyl, fluorenyl.

[0015] Preferably, the R 3 -R 4 The following groups are independently selected from methyl, ethyl, cyclopentyl, cyclohexyl, unsubstituted or substituted by Ra: phenyl, biphenyl, terphenyl, naphthyl, phenanthryl, triphenylene, fluorenyl, benzofuranyl, dibenzofuranyl, benzothienyl, dibenzothienyl, 9,9-dimethylfluorenyl, spirofluorenyl, arylamine, carbazolyl.

[0016] Preferably, Ar1-Ar4 are independently selected from the following groups which are unsubstituted or substituted by Ra: phenyl, biphenyl, terphenyl, naphthyl, phenanthryl, triphenylene, fluorenyl, benzofuranyl, dibenzofuranyl, benzothienyl, dibenzothienyl, 9,9-dimethylfluorenyl, spirofluorenyl, aromatic amine, and carbazole.

[0017] More preferably, the compound is selected from the following compounds A1-A30:

[0018]

[0019]

[0020] The second aspect of the present invention aims to provide an electron transport material comprising at least one of the compounds provided in the first aspect of the present invention.

[0021] The third aspect of the present invention aims to provide an organic electroluminescent device, which comprises at least one of the electron transport materials provided in the second aspect of the present invention.

[0022] The fourth aspect of the present invention aims to provide a display device, which comprises the organic electroluminescent device provided by the third aspect of the present invention.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The compound disclosed in the present invention has a parent structure of an acridine fused ring substituted aromatic amine, has high bond energy between atoms, has good thermal stability, is conducive to solid-state accumulation between molecules, has strong hole transition ability, and can be used as a hole transport layer material to effectively reduce device voltage and increase the life of the material.

[0025] The compound of the present invention is used in the hole transport layer, has a suitable energy level between adjacent layers, is conducive to the injection and migration of holes, can effectively reduce the driving voltage, and has a high hole migration rate, which can achieve good luminous efficiency in the device. The compound of the present invention has a large conjugated plane, is conducive to molecular stacking, exhibits good thermodynamic stability, and exhibits a long life in the device.

[0026] Meanwhile, the preparation process of the derivatives of the present invention is simple and easy, the raw materials are readily available, and the derivatives are suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only one embodiment of the present invention, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0028] Figure 1 This is a schematic diagram of the structure of a typical organic electroluminescent device. The components are: 1. substrate; 2. reflective anode electrode; 3. hole injection layer; 4. hole transport layer; 5. light-emitting layer; 6. electron transport layer; 7. electron injection layer; 8. cathode electrode. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0030] In the present invention, there is no particular limitation on the type and structure of the organic electroluminescent device, as long as the hole transport material provided by the present invention can be used.

[0031] The organic electroluminescent device of the present invention may be a light-emitting device of a top-emitting structure, for example, comprising an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a transparent or semi-transparent cathode in sequence on a substrate.

[0032] The organic electroluminescent device of the present invention may also be a bottom-emitting structure light-emitting device, for example, comprising a transparent or semi-transparent anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer and a cathode structure in sequence on a substrate.

[0033] The organic electroluminescent device of the present invention can also be a light-emitting device with a double-sided light-emitting structure, for example, a transparent or semi-transparent anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer and a transparent or semi-transparent cathode structure are sequentially included on a substrate.

[0034] In the organic electroluminescent device of the present invention, except for the hole transport layer comprising the hole transport material provided by the present invention, other layers may be made of any material used for the layers in the prior art.

[0035] Figure 1 A schematic diagram of a typical organic electroluminescent device is shown, wherein, from bottom to top, a substrate 1, a reflective anode electrode 2, a hole injection layer 3, a hole transport layer 4, a light-emitting layer 5, an electron transport layer 6, an electron injection layer 7, and a cathode electrode 8 are arranged in sequence.

[0036] Understandably, Figure 1 The structure of a typical organic electroluminescent device is schematically shown, and the present invention is not limited to this structure. The hole transport material of the present invention can be used in any type of organic electroluminescent device. For example, the organic electroluminescent device can also include an electron blocking layer, a hole blocking layer, a light extraction layer, etc. In actual application, these layers can be added or omitted according to specific circumstances.

[0037] For convenience, the following reference Figure 1The organic electroluminescent device of the present invention is described, but this does not mean any limitation on the protection scope of the present invention. It is understood that all organic electroluminescent devices that can use the hole transport material of the present invention are within the protection scope of the present invention.

[0038] In the present invention, the substrate 1 is not particularly limited, and conventional substrates used in organic electroluminescent devices in the prior art may be used, such as glass, polymer materials, and glass and polymer materials with TFT components.

[0039] In the present invention, the material of the reflective anode electrode 2 is not particularly limited, and can be selected from transparent conductive materials such as indium tin oxide (ITO), indium zinc oxide (IZO), tin dioxide (SnO2), zinc oxide (ZnO), low-temperature polycrystalline silicon (LTPS) known in the prior art, or metal materials such as silver and its alloys, aluminum and its alloys, or organic conductive materials such as PEDOT (poly 3,4-ethylenedioxythiophene), or a multilayer structure of the above materials.

[0040] In the present invention, the material of the hole injection layer 3 is not particularly limited, and hole injection materials known in the art or hole transport materials provided by the present invention can be selected as the hole injection material.

[0041] For example, the material of the hole injection layer may be selected from at least one of the following HT-1 to HT-31 compounds:

[0042]

[0043]

[0044] In the present invention, the hole injection layer 3 may further include a p-type dopant. The type of the p-type dopant is not particularly limited, and various p-type dopants known in the art may be used. For example, the p-type dopant may be selected from at least one of the following compounds:

[0045]

[0046] In the present invention, the amount of the p-type dopant is not particularly limited and may be an amount known to those skilled in the art.

[0047] In the present invention, the hole transport layer 4 comprises at least one of the hole transport materials of the present invention. The hole transport layer 4 may also comprise any combination of at least one of the hole transport materials of the present invention and known hole transport materials. Currently known hole transport materials may be selected from at least one of the above-mentioned HT-1 to HT-31 compounds, but are not limited to the above-mentioned compounds.

[0048] In the present invention, the luminescent material of the luminescent layer 5 is not particularly limited, and any luminescent material known to those skilled in the art can be used. For example, the luminescent material can include a host material and a guest material. For example, the known luminescent layer host material can be selected from at least one of the following GPH-1 to GPH-80 compounds:

[0049]

[0050]

[0051]

[0052] In a preferred embodiment of the present invention, the light-emitting layer 5 adopts phosphorescent electroluminescence technology. The guest material in the light-emitting layer 5 is a phosphorescent dopant, and the phosphorescent dopant can be selected from but not limited to one or more combinations of the following RPD-1 to RPD-28 compounds. The amount of the phosphorescent dopant is not particularly limited and can be an amount known in the art.

[0053]

[0054]

[0055] In the present invention, the material of the electron transport layer 6 is not particularly limited, and can be made of electron transport materials known in the art. For example, the electron transport layer material can be selected from at least one of the following compounds ET-1 to ET-57:

[0056]

[0057]

[0058]

[0059] In the present invention, the electron transport layer 6 may further include an n-type dopant, and the type of the n-type dopant is not particularly limited, and various n-type dopants known in the art may be used. For example, the n-type dopant may be a compound represented by the following formula:

[0060]

[0061] In the present invention, the amount of the n-type dopant is not particularly limited and can be an amount known to those skilled in the art.

[0062] In the present invention, the material of the electron injection layer 7 is not particularly limited, and electron injection materials known in the art can be used, for example, it can include but is not limited to at least one of the materials such as LiQ, LiF, NaCl, CsF, Li2O, Cs2CO3, BaO, Na, Li, Ca, etc. in the prior art.

[0063] In the present invention, the material of the cathode electrode 8 is not particularly limited, for example, it can be selected from but not limited to magnesium-silver mixture, LiF / Al, ITO, Al and other metals, metal mixtures, oxides and the like.

[0064] The display device of the present invention comprises the organic electroluminescent device of the present invention, including but not limited to a display, a television, a tablet computer, a mobile communication terminal, etc.

[0065] The method for preparing the organic electroluminescent device of the present invention is not particularly limited, and any method known in the art may be used. For example, the present invention may be prepared by the following preparation method:

[0066] (1) cleaning the reflective anode electrode 2 on the top-emitting OLED device substrate 1 by using a cleaning machine through steps such as chemical cleaning, water cleaning, brushing, high-pressure water cleaning, and air knife cleaning, and then performing a heat treatment;

[0067] (2) vacuum evaporating a hole injection material on the reflective anode electrode 2 to form a hole injection layer 3;

[0068] (3) vacuum evaporating a hole transport material on the hole injection layer 3 to form a hole transport layer 4;

[0069] (4) vacuum evaporating a light-emitting layer 5 on the hole transport layer 4, wherein the light-emitting layer 5 contains a host material and a guest material;

[0070] (5) vacuum evaporating an electron transport material on the light emitting layer 5 to form an electron transport layer 6;

[0071] (6) vacuum evaporating an electron injection material on the electron transport layer 6 as an electron injection layer 7, wherein the electron injection material is selected from one or a combination of materials such as LiQ, LiF, NaCl, CsF, Li2O, Cs2CO3, BaO, Na, Li, Ca, etc.;

[0072] (7) A cathode material is vacuum-deposited on the electron injection layer 7 to form a cathode electrode 8 .

[0073] The above only describes a typical structure of an organic electroluminescent device and its preparation method. It should be understood that the present invention is not limited to this structure. The hole transport material of the present invention can be used in an organic electroluminescent device of any structure, and the organic electroluminescent device can be prepared by any preparation method known in the art.

[0074] The synthesis method of the compound of the present invention is not particularly limited, and any method known to those skilled in the art can be used for synthesis. The following examples illustrate the synthesis process of the compound of the present invention.

[0075] Synthesis Example 1: Synthesis of Compound A1

[0076]

[0077] Add 100 mmol of aniline, 100 mmol of methyl 2-bromo-5-chlorobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M1.

[0078] Add 100 mmol of M1 and 200 ml of THF to the reaction flask, and add 220 mmol of methylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, then warm to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M2.

[0079] Add 100 mmol of M2 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M3.

[0080] Add 100 mmol of M3, 100 mmol of methyl 2-bromobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone palladium) (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4.

[0081] Add 100 mmol of M4 and 200 ml of THF to the reaction flask, and add 220 mmol of methylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, and then warm it to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M5.

[0082] Add 100 mmol of M5 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M6.

[0083] Add 100 mmol of aniline, 100 mmol of 2-bromo-9,9-dimethylfluorene, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M7.

[0084] Add 100 mmol of M6, 100 mmol of M7, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) into a reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A1.

[0085] 1 H NMR (400MHz, Chloroform) δ7.92-7.83(m,3H),7.53(d,J=7.6Hz,4H),7.33(d,J=11.2Hz,4H),7.21–7.06(m,6H),7.01-6.92(m,5H),1.66(s,18H).

[0086] M / Z: Exp., 608.5; Calc., 608.3.

[0087] Synthesis Example 2: Synthesis of Compound A5

[0088]

[0089] Add 100 mmol of aniline, 100 mmol of methyl 2-bromo-5-chlorobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M1.

[0090] Add 100 mmol of M1 and 200 ml of THF to the reaction flask, and add 220 mmol of methylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, then warm to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M2.

[0091] Add 100 mmol of M2 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M3.

[0092] Add 100 mmol of M3, 100 mmol of methyl 2-bromobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone palladium) (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4.

[0093] Add 100 mmol of M4 and 200 ml of THF to the reaction flask, and add 220 mmol of methylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, and then warm it to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M5.

[0094] Add 100 mmol of M5 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M6.

[0095] Add 100 mmol of aniline, 100 mmol of 4-bromobiphenyl, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M7.

[0096] Add 100 mmol of M6, 100 mmol of M7, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) into a reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A5.

[0097] 1 H NMR (400MHz, Chloroform) δ7.75-7.62(m,3H),7.46–7.41(m,5H),7.36(d,J=10.0Hz,3H),7.24–7.16(m,4H),7.11–6.86(m,9H),1.68(s,12H).

[0098] M / Z: Exp., 568.1; Calc., 568.3.

[0099] Synthesis Example 3: Synthesis of Compound A13

[0100]

[0101] Add 100 mmol of aniline, 100 mmol of methyl 2-bromo-5-chlorobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M1.

[0102] Add 100 mmol of M1 and 200 ml of THF to the reaction flask, and add 220 mmol of methylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, then warm to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M2.

[0103] Add 100 mmol of M2 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux to react for 12 hours. After the reaction is completed, add water, solid precipitates, filter and dry to obtain intermediate M3.

[0104] Add 100 mmol of M3, 100 mmol of methyl 2-bromobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone palladium) (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4.

[0105] Add 100 mmol of M4 and 200 ml of THF to the reaction flask, and add 220 mmol of phenylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, then warm to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M5.

[0106] Add 100 mmol of M5 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M6.

[0107] Add 100 mmol of aniline, 100 mmol of 2-bromo-9,9-dimethylfluorene, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M7.

[0108] Add 100 mmol of M6, 100 mmol of M7, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to a reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A13.

[0109] 1 H NMR(400MHz,Chloroform)δ7.85-7.78(m,3H),7.52(d,J=7.6Hz,3H),7.40-7.28(m,6H),7.25–7.15(m,8H),7.10(t,J=11.2Hz,3H),7.04 -6.91(m,9H),1.70(s,12H).

[0110] M / Z: Exp., 732.6; Calc., 732.3.

[0111] Synthesis Example 4: Synthesis of Compound A16

[0112]

[0113] Add 100 mmol of aniline, 100 mmol of methyl 2-bromo-5-chlorobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M1.

[0114] Add 100 mmol of M1 and 200 ml of THF to the reaction flask, and add 220 mmol of methylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, then warm to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M2.

[0115] Add 100 mmol of M2 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux to react for 12 hours. After the reaction is completed, add water, solid precipitates, filter and dry to obtain intermediate M3.

[0116] Add 100 mmol of M3, 100 mmol of methyl 2-bromobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone palladium) (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4.

[0117] Add 100 mmol of M4 and 300 ml of trifluoromethanesulfonic anhydride into the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M5.

[0118] 100mmol titanium tetrachloride was added to the reaction bottle, cooled to -40 degrees Celsius, 100mmol dimethyl zinc was added, the temperature was controlled and stirred for 30 minutes, and a solution of 100mmol M5 dissolved in 500ml dichloromethane was added dropwise. After the addition was completed, the temperature was controlled and reacted for 30 minutes, and the temperature was naturally raised to room temperature, and the reaction was stirred for 8 hours. Water was added to the reaction solution, extracted with dichloromethane, the organic phase was concentrated, and separated by silica gel column chromatography to obtain M6.

[0119] Add 100 mmol of aniline, 100 mmol of 2-bromo-9,9-dimethylfluorene, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M7.

[0120] Add 100 mmol of M6, 100 mmol of M7, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) into a reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A16.

[0121] 1H NMR(400MHz,Chloroform)δ7.88(d,J=10.0Hz,2H),7.53(d,J=8.8Hz,2H),7.37-7.2 9(m,4H),7.24(d,J=8.4Hz,2H),7.16–7.05(m,5H),7.00-6.85(m,7H),1.71(s,18H).

[0122] M / Z: Exp., 608.5; Calc., 608.3.

[0123] Synthesis Example 5: Synthesis of Compound A18

[0124]

[0125] Add 100 mmol of p-chloroaniline, 100 mmol of methyl 2-iodo-5-bromobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetonepalladium) (Pd(dba)) to a reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M1.

[0126] Add 100 mmol of M1 and 200 ml of THF to the reaction flask, and add 220 mmol of methylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, then warm to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M2.

[0127] Add 100 mmol of M2 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M3.

[0128] Add 100 mmol of M3, 100 mmol of methyl 2-bromobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone palladium) (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4.

[0129] Add 100 mmol of M4 and 300 ml of trifluoromethanesulfonic anhydride into the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M5.

[0130] 100mmol titanium tetrachloride was added to the reaction bottle, cooled to -40 degrees Celsius, 100mmol dimethyl zinc was added, the temperature was controlled and stirred for 30 minutes, and a solution of 100mmol M5 dissolved in 500ml dichloromethane was added dropwise. After the addition was completed, the temperature was controlled and reacted for 30 minutes, and the temperature was naturally raised to room temperature, and the reaction was stirred for 8 hours. Water was added to the reaction solution, extracted with dichloromethane, the organic phase was concentrated, and separated by silica gel column chromatography to obtain M6.

[0131] Add 100 mmol of aniline, 100 mmol of 2-bromo-9,9-dimethylfluorene, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M7.

[0132] Add 100 mmol of M6, 100 mmol of M7, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) into a reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M8.

[0133] Add 100 mmol of M8, 100 mmol of diphenylamine, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to a reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A18.

[0134] 1 H NMR(400MHz,Chloroform)δ7.91-7.85(m,2H),7.53(d,J=7.6Hz,3H),7.42-7.30(m,7H),7. 21(t,J=10.0Hz,3H),7.11(d,J=9.6Hz,5H),7.05-6.94(m,11H),1.83(s,6H),1.68(s,12H).

[0135] M / Z: Exp., 775.5; Calc., 775.4.

[0136] Synthesis Example 6: Synthesis of Compound A26

[0137]

[0138] Add 100 mmol of aniline, 100 mmol of methyl 2-bromo-4-chlorobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M1.

[0139] Add 100 mmol of M1 and 200 ml of THF to the reaction flask, and add 220 mmol of methylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, then warm to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M2.

[0140] Add 100 mmol of M2 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M3.

[0141] Add 100 mmol of M3, 100 mmol of methyl 2-bromobenzoate, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone palladium) (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4.

[0142] Add 100 mmol of M4 and 200 ml of THF to the reaction flask, and add 220 mmol of methylmagnesium bromide dropwise at 0°C. After the addition is complete, control the temperature to react for 1 hour, and then warm it to room temperature to react for 12 hours. After the reaction is complete, add water, extract with ethyl acetate, separate the organic phase, concentrate, and purify by column chromatography to obtain intermediate M5.

[0143] Add 100 mmol of M5 and 300 ml of glacial acetic acid to the reaction flask, heat and reflux for 12 hours. After the reaction is complete, add water, solid precipitates, filter and dry to obtain intermediate M6.

[0144] Add 100 mmol of M6, 100 mmol of 2-amino-9,9-dimethylfluorene, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M7.

[0145] Add 100 mmol of diphenylamine, 100 mmol of p-chlorobromobenzene, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to the reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M8.

[0146] Add 100 mmol of M7, 100 mmol of M8, 28.83 g of sodium tert-butoxide (300 mmol), 800 ml of xylene, and 1 mmol of bis(dibenzylideneacetone) palladium (Pd(dba)) to a reaction flask. React at 120°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A26.

[0147] 1 H NMR(400MHz,Chloroform)δ7.92-7.86(m,3H),7.52(d,J=7.6Hz,2H),7.32–7.21(m,6H),7.21–7.12( m,8H),7.09(d,J=10.0Hz,4H),7.00-6.92(m,6H),6.83(d,J=8.0Hz,2H),1.87(s,6H),1.69(s,12H).

[0148] M / Z: Exp., 775.2; Calc., 775.4.

[0149] Other compounds of the present invention can be synthesized by selecting appropriate raw materials according to the ideas of the above-mentioned synthesis examples 1-6, or by selecting any other appropriate method and raw materials for synthesis.

[0150] Example 1

[0151] The glass substrate coated with the ITO transparent conductive layer was ultrasonically treated in a commercial cleaning agent, rinsed in deionized water, ultrasonically degreased in an acetone-ethanol mixed solvent, baked in a clean environment to completely remove the moisture, cleaned with ultraviolet light and ozone, and bombarded with a low-energy cation beam;

[0152] Place the glass substrate with the anode in a vacuum chamber and evacuate the chamber to a pressure less than 10 -5 HT-11 was vacuum-deposited on the anode layer as a hole injection layer at a deposition rate of 0.1 nm / s and a deposition film thickness of 10 nm;

[0153] Vacuum evaporate A1 material on the hole injection layer as a hole transport layer, with an evaporation rate of 0.1 nm / s and an evaporation film thickness of 80 nm;

[0154] A light-emitting layer is vacuum-deposited on the hole transport layer. The light-emitting layer includes a main material GHP-15 and a dye material RPD-1. The deposition is performed by a multi-source co-evaporation method. The deposition rate of the main material GHP-15 is adjusted to 0.1 nm / s, and the deposition rate of the dye RPD-1 is adjusted to 3% of the deposition rate of the main material. The total deposition film thickness is 30 nm.

[0155] An electron transport layer is vacuum-deposited on the light-emitting layer. ET-42 is selected as the electron transport material. The evaporation rate is 0.1 nm / s and the evaporation film thickness is 30 nm.

[0156] LiF with a thickness of 0.5 nm was vacuum-deposited on the electron transport layer (ETL) as an electron injection layer at a rate of 0.1 nm / s;

[0157] Finally, an aluminum layer with a thickness of 150 nm was evaporated on the electron injection layer as a cathode of the organic electroluminescent device, and the evaporation rate was 0.1 nm / s.

[0158] Embodiment 2-6

[0159] Except that A5, A13, A16, A18 and A26 are used to replace A1 respectively, the rest is the same as Example 1.

[0160] Comparative Example 1

[0161] Except that HT-27 was used instead of A1, the rest was the same as Example 1.

[0162] The organic electroluminescent device prepared by the above process was subjected to the following performance tests:

[0163] At the same brightness, the driving voltage and current efficiency of the organic electroluminescent devices prepared in the embodiment and the comparative example and the life of the device were measured using a digital source meter and a brightness meter. Specifically, the voltage was increased at a rate of 0.1 V per second to measure the brightness of the organic electroluminescent device when it reached 5000 cd / m 2 The voltage at which the light is on is the driving voltage, and the current density at this time is measured at the same time; the ratio of brightness to current density is the current efficiency; the life test of LT95 is as follows: use a brightness meter at 5000cd / m 2 At the same brightness, the current is kept constant and the brightness of the organic electroluminescent device is measured to drop to 4750cd / m 2 The time is in hours. The test results are shown in Table 1.

[0164] Table 1. Organic electroluminescent device performance results

[0165]

[0166]

[0167] From the data in Table 1, it can be seen that the compound prepared in the present invention is used as a hole transport material for an organic electroluminescent device, which can effectively reduce the driving voltage, improve the current efficiency, and extend the life of the device, and is a hole transport material with good performance.

[0168] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. An acridine fused ring substituted aromatic amine compound, characterized in that: Having a structure as shown in formula (I): in, R 1 -R 2 independently selected from C1-C3 alkyl, C3-C6 cycloalkane, C6-C 30 Aromatic groups; R 3 -R 4 independently selected from C1-C3 alkyl, C3-C6 cycloalkane, C6-C 30 The aromatic group, and the adjacent substituents can be connected to form a ring; Ar1-Ar4 are independently selected from C6-C 30 Aromatic or C3-C 30 heteroaryl; m, n are selected from 0 or 1, and cannot be 0 at the same time; The heteroatoms on the heteroaryl group are each independently selected from O, S or N; The hydrogen atoms on the aromatic and heteroaryl groups may be independently substituted by Ra, wherein Ra is independently selected from deuterium, halogen, nitro, cyano, C1-C4 alkyl, C5-C 20 Cycloalkyl, phenyl, biphenyl, terphenyl or naphthyl.

2. The compound according to claim 1, characterized in that The R 1 -R 2 are independently selected from the following groups which are unsubstituted or substituted by Ra: methyl, ethyl, cyclopentyl, cyclohexyl, phenyl, biphenyl, naphthyl, phenanthrenyl, fluorenyl.

3. The compound according to claim 1, characterized in that The R 3 -R 4 The following groups are independently selected from methyl, ethyl, cyclopentyl, cyclohexyl, unsubstituted or substituted by Ra: phenyl, biphenyl, terphenyl, naphthyl, phenanthryl, triphenylene, fluorenyl, benzofuranyl, dibenzofuranyl, benzothienyl, dibenzothienyl, 9,9-dimethylfluorenyl, spirofluorenyl, arylamine, carbazolyl.

4. The compound according to claim 1, characterized in that The Ar1-Ar4 are independently selected from the following groups which are unsubstituted or substituted by Ra: phenyl, biphenyl, terphenyl, naphthyl, phenanthryl, triphenylene, fluorenyl, benzofuranyl, dibenzofuranyl, benzothienyl, dibenzothienyl, 9,9-dimethylfluorenyl, spirofluorenyl, arylamine, carbazolyl.

5. The compound according to claim 1, characterized in that It is selected from the compounds shown in the following A1-A30:

6. A hole transport material, characterized in that It comprises at least one of the compounds according to any one of claims 1 to 5.

7. An organic electroluminescent device, characterized in that: It contains at least one of the hole transport materials of claim 6.

8. A display device, characterized in that: It comprises the organic electroluminescent device according to claim 7.