A self-healing elastomer based on imidazole urea bond coordinated by copper ions

By designing imidazolour bonds based on copper ion coordination in self-healing elastomers and combining multiple dynamic bonds to construct Cu-BIMU locking units, the contradiction between tensile strength and self-healing ability in the prior art is solved. The combination of high tensile strength and high self-healing ability is achieved, and the tensile strength reaches 65.3MPa.

CN115926109BActive Publication Date: 2024-11-22DONGHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211304206.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-24
Publication Date
2024-11-22
Estimated Expiration
2042-10-24

AI Technical Summary

Technical Problem

Existing self-healing elastomers are difficult to have both high tensile strength and good self-healing ability. The strength and reversibility of dynamic bonds are usually negatively correlated, resulting in the construction of dynamic bonds that are both high-intensity and high-reversibility. A challenge.

Method used

Using imidazolium urea bond design based on copper ion coordination, the Cu-2,2-(imidazol-2-yl)-methaneurea (Cu-BIMU) locking unit is constructed by dynamic multi-bond coupling, combining dynamic covalent imidazole Urea bonds and non-covalent bonds (coordination bonds, π-π stacking bonds and hydrogen bonds) form super-strong self-healing elastomers with high comprehensive bond energy.

Benefits of technology

The high flowability and high reversibility of the polymer chain are achieved, and the tensile strength and self-healing ability of the elastomer are significantly improved. The tensile strength reaches 65.3MPa, exceeding the historical highest value of self-healing elastomers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115926109B_ABST
    Figure CN115926109B_ABST
Patent Text Reader

Abstract

The present invention relates to a self-healing elastomer based on imidazole urea bond coordinated by copper ions. The structural formula of the self-healing elastomer is (Ⅰ), (Ⅱ) or (Ⅲ). The self-healing elastomer is constructed by a Cu-BIMU locking unit coupled with a new dynamic imidazole urea bond and multiple non-covalent bonds. Cu-BIMU concentrates quadruple dynamic bonds in one locking unit instead of forming covalent or non-covalent cross-linking bonds that are usually independent of each other, so as to avoid forming too many apparent cross-linking sites, thereby ensuring the high fluidity of the polymer chain. At the same time, the coupled quadruple dynamic bonds construct an ultra-strong Cu-BIMU unit, while showing high comprehensive bond energy and reversibility, which helps to solve the long-standing contradiction between the high tensile strength and self-healing performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of self-healing materials, and in particular relates to an imidazole urea bond self-healing elastomer based on copper ion coordination. Background Art

[0002] Elastomers are one of the most consumed materials in daily life and have a wide range of applications. The global annual consumption of rubber was 28.98 million tons in 2019. They are increasingly important in key areas such as medical devices, aerospace, and soft robotics. However, elastomers are often damaged by external forces during their service life, which can significantly degrade their performance, shorten their service life, and pose serious safety risks. Self-healing is an attractive way to address these problems. Self-healing materials have received extensive attention in the past few decades. A major strategy for designing self-healing materials is to introduce reversible bonds into the polymer network. This approach improves the reliability of elastomers and enables them to heal multiple times. However, the fabrication of intrinsically self-healing elastomers with ultra-high tensile strength remains a key challenge. The tensile strength of most self-healing elastomers is limited to 10MPa. Common methods to improve the tensile strength of elastomers usually involve increasing the number of cross-linking sites, which, however, significantly hinders the mobility of the polymer chains and thus impairs their self-healing ability. In addition, the reversibility of dynamic bonds plays a key role in the self-healing process of elastomers. Many dynamic covalent bonds (such as Diels-Alder reactions, imine bonds, boron-oxygen bonds, and disulfide bonds) and non-covalent bonds (such as hydrogen bonds, coordination bonds, and π-π stacking bonds) are used to design self-healing materials. However, the strength and reversibility of dynamic bonds are usually negatively correlated. Therefore, it is a very challenging task to construct dynamic bonds or groups with both high strength and high reversibility. In general, high tensile strength and healing ability are often mutually exclusive. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a self-healing elastomer based on imidazole urea bond coordinated by copper ions, so as to overcome the problem that the self-healing elastomer in the prior art cannot have both good tensile strength and healing ability.

[0004] The present invention provides a super strong self-healing elastomer, the structural formula of which is as follows:

[0005]

[0006]

[0007] In the formula, m=any integer between 1 and 30, n=any integer between 1 and 30, and x=any integer between 1 and 30.

[0008] The present invention also provides a method for preparing a super strong self-healing elastomer, comprising:

[0009] (1) under nitrogen atmosphere, diphenylmethane diisocyanate (MDI) is added to polytetramethylene glycol (PTMG) for the first nucleophilic addition reaction, and after cooling, 2,2-diimidazole methane and a solvent are added for the second nucleophilic addition reaction, and the obtained solution is added dropwise to ether to generate precipitation, and dried to obtain a polyurethane based on imidazole urea bonds;

[0010] (2) The polyurethane based on imidazole urea bond in step (1) is mixed with a solvent to obtain a polyurethane solution based on imidazole urea bond, copper salt is mixed with the solvent to obtain a copper salt solution, the two solutions are mixed and cast into a mold, the solvent is volatilized, and the mixture is dried to obtain a super strong self-healing elastomer.

[0011] Preferably, in step (1), the molar ratio of MDI, PTMG and 2,2-diimidazole methane is 1.9-2.1:0.9-1.1:0.9-1.1.

[0012] Preferably, in step (1), the ratio of 2,2-diimidazole methane to solvent is 1 mmol:10-12 mL.

[0013] Preferably, the solvent in step (1) is DMF; and MDI includes 2,4-MDI and / or 4,4′-MDI.

[0014] Preferably, the temperature of the first nucleophilic addition reaction in step (1) is 100-120° C. and the time is 1-3 h.

[0015] Preferably, the temperature of the second nucleophilic addition reaction in step (1) is 70-80° C. and the time is 20-30 h.

[0016] Preferably, in step (2), the mass ratio of the polyurethane based on the imidazole urea bond to the copper salt is 100:0.001 to 100:5.

[0017] Preferably, in step (2), the concentration of the polyurethane solution based on imidazole urea bonds is 0.1-0.5 g / mL; and the concentration of the copper salt solution is 0.01-0.02 g / mL.

[0018] Preferably, the solvent in step (2) comprises one or more of tetrahydrofuran and acetone; the copper salt comprises one or more of copper hydrochloride, copper sulfate, copper bromide, copper acetate, copper nitrate, copper citrate, copper methanesulfonate, copper acetylacetate, copper fluoroborate, copper difluoride, copper gluconate, basic copper carbonate, copper sulfide, copper thiocyanate, copper iodide, copper niobate, copper ethoxide, copper phosphate, copper oxalate, copper trifluoroacetate, copper tetraethyl cyanide hexafluorophosphate, copper pyrophosphate, copper stearate, bis(trifluoromethanesulfonic acid)imide copper, and copper trifluoromethanesulfonate.

[0019] Preferably, in step (2), the volatile solvent is volatilized at room temperature for 20-30 hours; and the drying is dried under vacuum conditions at 55-65°C.

[0020] The invention also provides an application of a super strong self-healing elastomer in coatings, leather or biomedical materials.

[0021] This paper proposes a new molecular strategy, namely dynamic multi-bond coupling locking units, rather than typical independent covalent or non-covalent cross-linking, to construct ultra-strong self-healing elastomers ( Figure 1 a). The key is the Cu-2,2-(imidazol-2-yl)-methaneurea (Cu-BIMU) locking unit, which locks the newly designed dynamic covalent imidazole urea bond and triple dynamic non-covalent bonds (coordination bond, π-π stacking bond and hydrogen bond) into one unit ( Figure 1 b), Figure 1 The Cu-BIMU locked unit in b is composed of reversible imidazole urea bonds (green arrows and gray sticks), copper ion coordination (gradient gray sticks and orange disks; the gray gradient indicates the electron cloud density gradient caused by the electron-withdrawing properties of copper ions), hydrogen bonds (blue equal signs), and π-π stacking bonds (purple equal signs) form a dynamic network. The coupled quadruple dynamic bonds construct an ultra-strong Cu-BIMU unit with high comprehensive bond energy, thus forming a Cu-BIMU polyurethane (Cu-BIMU-PU) elastomer with ultra-high tensile strength. Self-healing properties are generally related to the mobility of polymer chains and the reversibility of cross-linking sites. The quadruple dynamic bonds are locked in the Cu-BIMU unit to avoid the formation of too many cross-linking sites, thereby ensuring sufficient mobility of the polymer chains in Cu-BIMU PU. At the same time, the locked quadruple dynamic bonds with synergistic effects have high reversibility. 2,2-Diimidazole methane (BIM) reacts with isocyanate to form dynamic imidazole urea bonds, hydrogen bonds, and π-π stacking bonds. The electron cloud of the nitrogen atom in the imidazole ring of the imidazole-urea bond is relatively lower than that of normal aliphatic amines ( Figure 1 c), resulting in high reversibility of the urea bond. The coordination of copper ions with BIM further reduces the electron cloud density of the nitrogen atom in the urea bond through the conjugated structure of the imidazole ring, thereby enhancing the reversibility of the BIMU bond. Overall, the design of the locking unit with synergistic multiple dynamic covalent and non-covalent bonds simultaneously ensures high tensile strength and self-healing ability.

[0022] Beneficial Effects

[0023] The present invention designs a new dynamic imidazole urea bond and multiple non-covalent bond coupled Cu-BIMU locking unit to construct a high-performance self-healing elastomer. Cu-BIMU concentrates quadruple dynamic bonds in one locking unit, rather than forming covalent or non-covalent cross-linking bonds that are usually independent of each other, to avoid the formation of too many apparent cross-linking sites, thereby ensuring high fluidity of the polymer chain. At the same time, the coupled quadruple dynamic bonds construct an ultra-strong Cu-BIMU unit while showing high comprehensive bond energy and reversibility. This new molecular design of locking units with coupled multiple bonds and multiple cross-links in a single site topology helps to solve the long-standing contradiction between the high tensile strength and self-healing properties of the material. The tensile strength of the resulting polyurethane is 65.3MPa, which is the highest value ever for a self-healing elastomer. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Design of Cu-BIMU polyurethane elastomer with super self-healing properties, a) Molecular structure of Cu-BIMU-PU elastomer, b) Schematic diagram of BIMU-PU elastomer structure, c) Schematic diagram of electron transfer among normal urea bonds, BIMU bonds and Cu-BIMU bonds.

[0025] Figure 2 Figure 2 shows the dynamic exchange reaction in a small molecule model containing an imidazole urea bond. a) The exchange reaction between a and b generates c and d using isocyanate e as an intermediate. b) 1H NMR spectra of a and b after mixing at 25°C for different time periods. c) The conversion rate of b when equilibrium is reached in the absence of CuCl2 (conversion rate = ([b]0-[b] t ) / ([b]0-[b] eq ), [b]0 = initial concentration of b, [b] t = the concentration of b at time t, [b] eq = equilibrium concentration of b), d) 1H NMR spectra after mixing a, b and CuCl2 at 25°C for different times, e) conversion rate of b when equilibrium is reached in the presence of CuCl2 (conversion rate = ([b]0-[b] t ) / ([b]0-[b] eq ).

[0026] Figure 3 The in situ 1 H NMR ( 1 H NMR) spectroscopy.

[0027] Figure 4Free energy diagrams for the conversion of B(BIM) to ABA(BIMU) with (right) and without (left) Cu2+ coordination. The geometries of the initial state (IS), transition state (TS), and final state (FS) of the rate determining step (RDS) in the first and second steps are shown above and below the free energy diagrams, respectively.

[0028] Figure 5 Bader charge analysis diagrams of N and H in A+B (a) and A+B-CuCl2 (b).

[0029] Figure 6 Electron localization functions (ELFs) of AB and AB-CuCl2, where (a) N1-H represents TS1 and TS3, (b) N2-H represents TS1 and TS3, (c) N1-H represents TS2 and TS4, and (d) N2-H represents TS2 and TS4.

[0030] Figure 7 This is the hydrogen NMR spectrum of BIMU-PU.

[0031] Figure 8 Fourier transform infrared spectra of BIMU-PU and Cu-BIMU-PU.

[0032] Fig. 9 In-situ variable temperature FTIR spectrum of BIMU-PU.

[0033] Fig.10 Cu 2+ Effect of coordination on the dynamic, mechanical and thermal properties of Cu-BIMU-PU network, a) In situ variable temperature FTIR spectrum of Cu-BIMU-PU, b) DSC curves of BIMU-PU and Cu-BIMU-PU samples, c) Storage modulus (G′) and loss modulus (G′) of Cu-BIMU-PU as a function of temperature, d) Tensile stress-strain curves of BIMU-PU and Cu-BIMU-PU, e) Continuous cyclic tensile curves of Cu-BIMU-PU at different strains without waiting time between two consecutive loadings, f) Repeated cyclic tensile curves of Cu-BIMU-PU at 100% strain. From cycle 1 to cycle 10, there is no waiting time in between. Next, the dumbbell-shaped sample was relaxed at room temperature for 12 h before the 11th cyclic tensile test.

[0034] Fig.11 BIMU-PU and Cu-BIMU-PU in air at 20℃·min -1 TGA curve of .

[0035] Fig.12 Storage modulus (G′) and loss modulus (G′) of BIMU-PU vary with temperature.

[0036] Fig.13 Comparison of toughness of BIMU-PU and Cu-BIMU-PU.

[0037] Fig.14 Sequential cyclic tensile curves of BIMU-PU at different strains, with no waiting time between two consecutive loadings.

[0038] Fig.15 This is the repeated cyclic tensile curve of BIMU-PU.

[0039] Fig.16 Healing properties of Cu-BIMU-PU, a) tensile stress-strain curves of original and healed Cu-BIMU PU (healed at 100°C for 12 h), b) Ashby plot of tensile strength of Cu-BIMU-PU and other self-healing elastomers reported in existing literature, c) Cu-BIMU-PU film cut in half, reconnected and healed at 100°C for 12 h can lift a 20.41 kg (about 80,000 times its own weight) bucket, d) optical microscope images of scratches on the Cu-BIMU-PU film before and after healing at 100°C for 2 h, e) XPS spectra of BIMU-PU and Cu-BIMU-PU in the N1s region, f) XPS spectrum of Cu-BIMU-PU in the cu2p region.

[0040] Fig.17 Tensile stress-strain curves of original and healed (100℃, 12h) BIMU-PU. DETAILED DESCRIPTION

[0041] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0042] Sources of reagents: 2,2-diimidazole methane (BIM, 97%) was purchased from Beijing Huawei Ruike Chemical (China). CuCl2 (99%), n-hexane and anhydrous ether were purchased from Sinopharm Chemical Reagent (China). PTMG (Mn = ~1000 g mol-1) and 2-ethylimidazole (98%) were purchased from Aladdin (China). MDI (2,4-MDI / 4,4′-MDI = 50 / 50, 99.6%) was purchased from Wanhua Chemical (China). Anhydrous tetrahydrofuran (THF) and N,N-dimethylformamide (DMF) were purchased from J&K Scientific (China). Propyl isocyanate was purchased from Jiuding Chemical (China). Phenethyl isocyanate was purchased from Adamas (China).

[0043] Characterization and Testing:

[0044] Characterization and measurement of 1H-NMR spectra were recorded using a Bruker Avance 600NMR spectrometer. Chemical shifts (δ) were reported in ppm relative to the residual solvent signal (deuterated tetrahydrofuran (THF-d8): 1.76 and 3.61 ppm). FTIR spectra were recorded on a Nicolet 8700 spectrometer (Thermo Electron Corporation). Spectra were collected by 32 scans with a spectral resolution of 4 cm-1 and a wavenumber range of 4000-500 cm-1. Uniaxial tensile tests were performed at a tensile rate of 100 mm min-1 on an electronic universal testing machine (Changchun Kexin Testing Instrument Co., Ltd., WDW3020). Cyclic tensile tests were performed on a testing machine (Exceed E42) with a 100-N load cell at a tensile rate of 100 mm min-1 and a recovery rate of 20 mm min-1. Gel permeation chromatography (GPC) was performed using an Agilent GPC 50, and dimethylacetamide (DMAC) was used as an eluent. Rheological tests were performed on a TA DHR-2 rotational rheometer at a heating rate of 5°C min-1, a frequency of 1.0 Hz, and a strain of 1%. TGA was performed on a NETZSCH Libra / 209F1 instrument at a heating rate of 10°C min-1 under a nitrogen atmosphere. DSC was performed using a differential scanning calorimeter (NETZSCH, DSC 204F1, China) at a heating rate of 5°C min-1 under a nitrogen atmosphere. XPS spectra were recorded using a Thermo Fisher Scientific Escalab 250Xi instrument, and profiles were analyzed using the Avantage software system. Rheological tests were performed using DHR (TA, USA). Storage modulus and loss modulus were monitored at a frequency of 1.0 Hz and a heating rate of 5°C min-1.

[0045] Example 1

[0046] Synthesis route of Cu-BIMU-PU:

[0047]

[0048] Synthesis of BIMU-PU: PTMG (25 g, 25 mmol) was added to a glass reactor equipped with a magnetic stirrer and vacuum dried at 110 ° C for 2 h. After cooling to 70 ° C, MDI (12.5 g, 50 mmol) was added dropwise to the reactor under a nitrogen atmosphere and heated to 110 ° C for 2 h. After cooling to 75 ° C, 2,2-diimidazole methane (3.7 g, 25 mmol) and DMF (265 mL) were added and reacted for 24 hours. The above solution was added dropwise to ether to produce a white precipitate, which was then dried to obtain BIMU-PU (Mn = 168624, PDI = 4.866 according to GPC measurement).

[0049] Synthesis of Cu-BIMU-PU:

[0050] BIMU-PU (12 g) was dissolved in 40 mL THF. CuCl2 (0.2448 g) was dissolved in 20 mL THF. The two solutions were mixed and cast into a polytetrafluoroethylene mold. The solvent was first evaporated at room temperature for 24 hours, and then the remaining solvent was removed from the sample under vacuum at 60 ° C.

[0051] The structure of BIMU-PU is 1 H NMR characterization ( Figure 7 ). CuCl2 was introduced into BIMU-PU to form a coordination bond between copper ions and imidazole, forming a Cu-BIMU-PU hybrid network. In Fourier transform infrared spectroscopy (FTIR) ( Figure 8 ), after adding CuCl2, 695cm -1 The peak at (corresponding to the stretching vibration of C–N in the imidazole unit) shifts to 687 cm -1 , indicating that there is a coordination bond between copper ions and imidazole in Cu-BIMU-PU elastomer.

[0052] Synthesis of small molecule model compound a

[0053]

[0054] 2-Ethylimidazole (compound e, 0.96 g, 10 mmol) was dissolved in acetone (5 mL). Phenethyl isocyanate (compound d, 1.47 g, 10 mmol) was added to react for 15 min under a nitrogen atmosphere at 50° C. The resulting precipitate was added to n-hexane to generate a white precipitate at −20° C. and dried under vacuum at room temperature to obtain compound a ((2-ethyl-N-phenethyl-1H-imidazole-1-carboxamide)).

[0055] Synthesis of small molecule model compound c

[0056] 2-Ethylimidazole (0.96 g, 10 mmol) was dissolved in acetone (5 mL). Propyl isocyanate (Compound b, 0.85 g, 10 mmol) was added to react for 6 h at 50 ° C under a nitrogen atmosphere. The solution was then added dropwise to n-hexane to generate a white precipitate at -20 ° C. The white precipitate was dried in vacuo at room temperature to obtain Compound c.

[0057] In order to study the reversibility of the BIMU bond, compound a, a small molecule model containing an imidazole-urea bond (2-ethyl-N-phenethyl-1H-imidazole-1-carboxamide), was synthesized and mixed with propyl isocyanate (compound b) in deuterated dimethyl sulfoxide. The chemical shifts used to distinguish different molecules were marked at the corresponding proton positions. The chemical shifts given in brackets are caused by the coordination of the copper ion with the imidazole ( Figure 2 a) A mixture of a and b 1 The proton signals at 3.47 ppm and 3.31 ppm in the HNMR spectrum correspond to the chemical shifts of the methylene groups near the nitrogen atoms of compounds a and b, respectively. Figure 2 b). As time goes by, two new proton signals at 3.18 and 3.57 ppm appear, corresponding to the chemical shifts of the nitrogen atoms of 2-ethyl-N-propyl-1H-imidazole-1-carboxamide (compound c) and phenethyl isocyanate (compound d), respectively. That is, the proton peak intensity of a and b gradually decreases over time, while the proton peak intensity of c and d gradually increases until equilibrium is reached at ~19h. This indicates that an exchange reaction has occurred. At 25°C, it takes nearly 19 hours to reach equilibrium ( Figure 2 c), while the reported sp3 nitrogen atoms based on dynamically hindered urea bonds require 20 hours to reach equilibrium at 37 °C. Therefore, it can be inferred that compared with conventional aliphatic amine sp 3 Compared with the nitrogen atom, the sp 2 The electron cloud of nitrogen atom is relatively low, which leads to high reversibility of urea bond. 1 H NMR ( 1 H NMR spectroscopy was used to reveal its dissociation reaction ( Figure 3), a proton peak appeared at 3.57ppm, and its intensity gradually increased, indicating the generation of compound d. A proton peak appeared at 2.65ppm, and its intensity gradually increased, indicating the generation of compound e, which shows that the dynamic exchange reaction of the imidazole-urea bond unit involves two steps. First, the imidazole-urea bond unit in compound a is decomposed into isocyanate groups in compound d and decomposed into imidazole groups in compound e. Compound e reacts with the isocyanate groups in compound b to form the imidazole-urea bond unit in compound c. These experiments clearly demonstrate the reversibility of the imidazole-urea bond, which can be used for the dynamic reconstruction of the BIMU-PU network.

[0058] DFT calculations

[0059] All density functional theory (DFT) calculations were performed with the Vienna Ab initio Simulation Package (VASP) using the Perdew-Burke-Ernzerhof (PBE) functional with the generalized gradient approximation (GGA). The projected augmented wave (PAW) potential was chosen to describe the ion core and valence electrons, and a plane wave basis set with a kinetic energy cutoff of 400 eV was used. The DFT-D3 empirical correction method was used to describe the van der Waals interactions. The geometry was optimized with a resolution of less than The force convergence of is carried out, where the same convergence is applied to localize the transition states through constrained optimization. In addition, a (1 × 1 × 1) k-point sampling with a gamma-centered scheme is used for the total energy calculation.

[0060] Density functional theory (DFT) calculations were performed using imidazole and methyl isocyanate as models, revealing the catalytic effect of CuCl2 (black line) compared with the case without CuCl2. Figure 4 ) in a two-step concerted reaction. In the first step, A (methyl isocyanate) and B (bis-(imidazol-2-yl)-methaneurea) react to form (2-((1H-imidazol-2-yl)methyl)-N-methyl-1H-imidazole-1-carboxamide), which involves the breaking of the N–H bond on B, accompanied by the formation of the C–N bond between A and B and the simultaneous transfer of H from B to A. In the absence of CuCl2, the barriers are approximately 1.644 and 1.692 eV, respectively. However, when CuCl2 is used, the barrier of the second concerted process is reduced by approximately 0.1 eV. This reveals the catalytic role of CuCl2 in the dynamic dissociation / association of BIMU bonds.

[0061] The charge distribution is also analyzed to understand its chemical origin. The electronic charge distribution is partitioned and assigned to individual atoms based on DFT calculations. The difference in the partitioned charges of N and H indicates the charge transfer between B and A, which helps determine the difficulty of bond formation and breaking. Bader charge analysis such as Figure 5As shown, it represents the difference in H or N charge between A+B and A+B-CuCl2. N atoms are negatively charged and H atoms are positively charged, which is consistent with the electronegativity of the two elements. After imidazole is coordinated with CuCl2, the polarity of the N–H bond increases, which promotes the transfer of H; thus, the energy barrier of the chemical reaction is reduced.

[0062] The electron localization functions (ELFs) were analyzed. ELFs can be used to quantify the strength of the electronic overlap and interaction between N and H in the transition state, such as Figure 6 The results show that when imidazole and CuCl2 are coordinated, N1 and H ( Figure 6 The distance between N1 and H in TS1 and TS2 is smaller than that in TS3 and TS4. However, when imidazole and copper ions are coordinated, the interaction between N2 and H between AB and AB-CuCl2 is weakened by 0.32 eV ( Figure 6 b), the interaction between ABA and ABA-CuCl2 is weakened by 0.12 eV ( Figure 6 d). Therefore, the addition of CuCl2 facilitates the breaking of H-N1 bonds and the formation of H-N2 bonds.

[0063] The thermal reversibility of the imidazole-urea bond in BIMU-PU and Cu-BIMU-PU was studied by in situ variable temperature FTIR spectroscopy. At 110℃, BIMU-PU began to emit a peak at 2275 cm -1 The FTIR signal of isocyanate group is shown at Fig. 9 ). When the temperature increases, the peak of the isocyanate group increases significantly, indicating the dissociation of the imidazole-urea bond. 2+ After coordination, Cu-BIMU-PU begins to show FTIR signals of isocyanate groups at lower temperatures (100 °C) ( Fig.10 ). These results indicate that the coordinated copper ions enhance the reversibility of the imidazole-urea bond in the polymer, which is consistent with the experimental results of the small molecule model. To study the effect of copper ions on the thermal properties of Cu-BIMU-PU, we performed thermogravimetric analysis (TGA), differential scanning calorimetry (DSC), and oscillatory rheological analysis. The TGA curve shows that the thermal decomposition temperature of Cu-BIMU-PU is 9°C lower than that of BIMU-PU, which may be due to the fact that the coordination of copper ions promotes the dynamic dissociation of the imidazole-urea bond ( Fig.11 ). Both BIMU-PU and Cu-BIMU-PU show a low glass transition temperature (BIMU-PU: T g =-29.7℃,Cu-BIMU-PU:T g = -29.3 °C), no crystallization or melting peak between -70 and 120 °C ( Fig.10 b) These results show that Cu 2+The introduction of coordination bonds did not increase the crosslink density. Therefore, Cu-BIMU can be designed to lock multiple bonds in one unit to avoid the formation of too many crosslinking sites. As a result, the Cu-BIMU-PU polymer chains exhibit high mobility, which is conducive to self-healing. The thermal properties of Cu-BIMU-PU and BIMU-PU were further evaluated by oscillatory rheological analysis. The oscillatory rheological curves with temperature showed that the storage modulus (G') of BIMU-PU dropped sharply from 120℃ ( Fig.12 ). When the temperature rises to about 140°C, G′ intersects with the loss modulus (G″), indicating that BIMU-PU enters a viscous flow state at 140°C. 2+ After coordination, G′ remains higher than G″ until about 190°C, indicating the high integrated bond energy of the locking unit in Cu-BIMU-PU, which remains highly elastic at 190°C ( Fig.10 c).

[0064] The mechanical properties of Cu-BIMU-PU and BIMU-PU were evaluated by tensile tests. 2+ After coordination, the mechanical properties are greatly improved. Compared with the tensile strength of BIMU-PU, the tensile strength of Cu-BIMU-PU increases from 7.3±0.3 to 65.3±1.4MPa ( Fig.10 d), increased by nearly 9 times, with its toughness increasing from 45.7±2.4 to 147.1±5.5 MJ m -3 ( Fig.13 The Cu-BIMU locking units with coupled quadruple dynamic bonds (including imidazole-urea bonds, coordination bonds, π-π stacking bonds, and hydrogen bonds) endow the elastomer with high toughness. Cyclic tensile tests were performed to further evaluate the mechanical properties. Continuous cyclic tensile tests with increasing strain were performed without any waiting time between two consecutive loadings ( Fig.10 e and Fig.14 ). As the strain increases, the residual strain of Cu-BIMU-PU also gradually increases, because the Cu-BIMU unit breaks during the stretching process and reforms at a new location. However, the maximum stress of BIMU-PU under large strain decreases significantly. Comparison of the above results shows that Cu 2+ The formation of coordination is relatively fast, which is the main reason for the high tensile strength. In addition, cyclic tensile tests at 100% strain were performed without any waiting time between two consecutive cyclic tests of 10 cycles ( Fig.10 f and Fig.15). Cu-BIMU-PU exhibits a large hysteresis loop in the first cycle, indicating significant energy dissipation. The energy dissipation in the second cycle is much smaller than that in the first cycle because the broken dynamic bonds do not have enough time to recover to their original state within a limited time. After 10 stretching cycles, the residual strain of Cu-BIMU-PU was 18%, while that of BIMU-PU was 34% (approximately twice that of Cu-BIMU-PU). After relaxation for 12h, the hysteresis loop recovery rate of Cu-BIMU-PU reached 84.5% of the original value (ratio of the hysteresis loop area before and after relaxation), which is much higher than that of BIMU-PU (54.9%). These results indicate that coordination bonds with high bond energy remain stable over a strain range of up to 100%, which facilitates the reorganization of broken adjacent weak bonds (including hydrogen bonds and π-π stacking bonds) in the Cu-BIMU locking unit. Therefore, Cu-BIMU-PU exhibits higher elasticity than BIMU-PU. These results indicate that Cu 2+ Greatly improves the mechanical and thermal properties of elastomers.

[0065] The self-healing properties of Cu-BIMU-PU were evaluated in detail. Fig.16 a), the Cu-BIMU-PU dumbbell-shaped sample was first cut into two pieces and then connected at 100 °C. After 12 h, its tensile strength recovered to 90.2% (58.9 ± 1.0 MPa) of the original stress (65.3 ± 1.4 MPa), which is higher than the original tensile strength of all reported self-healing elastomers ( Fig.16 b), the toughness recovered to 88.6% (130.40±1.1MJ m-3) of the original (147.1±5.5MJ m-3). -3 ). The coordination of copper ions plays a key role in this phenomenon. Before the formation of coordination, BIMU-PU can recover 94.5% (6.9±0.6MPa) of the original strength (7.3±0.3MPa) and the original toughness (45.5±2.2MJ m -3 ) of 94.1% (42.8±5.3 MJ m -3 )( Fig.17 ). This result shows that Cu 2+ The coordination bonds significantly enhance the strength of the elastomer while maintaining its high healing efficiency. In addition, after cutting, the Cu-BIMU-PU strip (width: 5 mm; thickness: 10 mm) can lift a heavy barrel (20.41 kg) weighing more than 80,000 times its own weight after healing at 100°C for 12 hours ( Fig.16 c). Surface scratch recovery test was also carried out ( Fig.16d). The Cu-BIMU-PU film was scratched using a blade. The optical microscope image showed that the film almost completely healed within 2 hours at 100 °C.

[0066] The self-healing behavior of a material is usually closely related to its surface structure. Therefore, narrow X-ray photoelectron spectroscopy (XPS) was used to analyze the surface chemistry of BIMU-PU and Cu-BIMU-PU. Fig.16 e and 16f), there are significant differences in N 1s before and after coordination, and the BIMU-PU peak at 399.9 eV is attributed to CN and C=N, respectively. 2+ After coordination, the Cu-BIMU-PU peak at 399.4 eV is attributed to CN and C=N, and the Cu-CN peak at 400.9 eV is attributed to Cu-CN. This is because Cu 2+ The ions on the coordinated N charge cloud are transferred to Cu 2+ , weakening the shielding effect of the outer electrons of the nitrogen atom. Therefore, the binding energy of the coordinated nitrogen increases from 399.4eV to 400.9eV. This phenomenon proves that Cu 2+ Coordination with imidazole can further reduce the electron cloud density of the imidazole ring, which is beneficial to the BIMU bond dynamics. The Cu 2p XPS spectrum of Cu-BIMU-PU is shown in Figure 2. Fig.16 f. The oscillation peaks at 940.1-947.3 and 961.1-964.5 eV indicate the presence of Cu 2+ The peak at 933.1eV is attributed to the Cu2+ complex, which is also consistent with the changes in FTIR. The peak at 934.7eV is attributed to Cu 2+ In ionic bonding, the exchange reaction of BIMU and Cu-BIMU units can be promoted, further promoting healing.

Claims

1. A super strong self-healing elastomer, characterized in that: The structural formula is as follows: In the formula, m=any integer between 1 and 30, n=any integer between 1 and 30, and x=any integer between 1 and 30.

2. A method for preparing a super strong self-healing elastomer, comprising: (1) adding diphenylmethane diisocyanate (MDI) to polytetramethylene glycol (PTMG) for the first nucleophilic addition reaction, cooling, adding 2,2-diimidazole methane and a solvent for the second nucleophilic addition reaction, dropping the obtained solution into ether to generate a precipitate, and drying to obtain a polyurethane based on an imidazole urea bond; (2) The polyurethane based on imidazole urea bond in step (1) is mixed with a solvent to obtain a solution of the polyurethane based on imidazole urea bond, copper salt is mixed with the solvent to obtain a copper salt solution, the two solutions are mixed and cast into a mold, the solvent is volatilized, and the mold is dried to obtain a super strong self-healing elastomer.

3. The preparation method according to claim 2, characterized in that: In the step (1), the molar ratio of MDI, PTMG and 2,2-diimidazole methane is 1.9-2.1:0.9-1.1:0.9-1.1; the ratio of 2,2-diimidazole methane to the solvent is 1 mmol:10-12 ml.

4. The preparation method according to claim 2, characterized in that: The solvent in step (1) is DMF; MDI includes 2,4′-MDI and / or 4,4′-MDI.

5. The preparation method according to claim 2, characterized in that: In the step (1), the first nucleophilic addition reaction temperature is 100-120° C. and the time is 1-3 h; the second nucleophilic addition reaction temperature is 70-80° C. and the time is 20-30 h.

6. The preparation method according to claim 2, characterized in that: In the step (2), the mass ratio of the polyurethane based on the imidazole urea bond to the copper salt is 100:0.001 to 100:5; the concentration of the polyurethane solution based on the imidazole urea bond is 0.1-0.5 g / mL; and the concentration of the copper salt solution is 0.01-0.02 g / mL.

7. The preparation method according to claim 2, characterized in that: The solvent in step (2) includes one or more of tetrahydrofuran and acetone; the copper salt includes one or more of copper hydrochloride, copper sulfate, copper bromide, copper acetate, copper nitrate, copper citrate, copper methanesulfonate, copper acetylacetate, copper fluoroborate, copper difluoride, copper gluconate, basic copper carbonate, copper sulfide, copper thiocyanate, copper iodide, copper niobate, copper ethoxide, copper phosphate, copper oxalate, copper trifluoroacetate, copper tetraethyl cyanide hexafluorophosphate, copper pyrophosphate, copper stearate, bis(trifluoromethanesulfonic acid)imide copper, and copper trifluoromethanesulfonate.

8. The preparation method according to claim 2, characterized in that: In the step (2), the solvent is volatilized at room temperature for 20-30 hours; and the drying is carried out under vacuum at 55-65°C.

9. Use of the super strong self-healing elastomer as claimed in claim 1 in coatings, leather or biomedical materials.