Composite lithium metal negative electrode material and preparation method and application thereof

By dispersing lithium metal particles in the carbon matrix and forming a lithium/carbon composite layer, the dendrites and volume expansion of metal lithium negative electrode materials are solved, and efficient lithium storage performance and cycle stability are achieved, which is suitable for the safety of lithium batteries. and service life is improved.

CN115939358BActive Publication Date: 2024-11-05BEIJING ELECTRIC VEHICLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310028701.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-11-05
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

Metal lithium anode materials are prone to dendrite and volume expansion during charging and discharging, resulting in reduced cycle life and safety issues. The existing improvement methods are difficult to effectively solve these problems.

Method used

Using composite lithium metal negative electrode material, the lithium/carbon composite layer is formed on the surface of the lithium metal particles by dispersing lithium metal particles and forming a lithium/carbon composite layer on the surface of the lithium metal particles, the generation and volume expansion of lithium dendrites are inhibited, and the circulation stability is improved. The material consists of a carbon matrix and lithium metal particles. The lithium metal particles are distributed on the inside and/or the surface of the carbon matrix. They are synthesized in an inert atmosphere by spraying to form spherical or bulky carbon matrix and lithium metal particles to ensure uniformity of the material and structural compactness.

Benefits of technology

It effectively improves the growth of lithium dendrites, slows down the volume expansion of lithium negative electrodes, improves lithium storage performance and cycle stability, is suitable for batch preparation, and improves the safety performance and service life of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115939358B_ABST
    Figure CN115939358B_ABST
Patent Text Reader

Abstract

The present invention discloses a composite lithium metal negative electrode material and a preparation method and application thereof. The composite lithium metal negative electrode material comprises a carbon matrix and lithium metal particles, wherein the lithium metal particles are distributed inside and / or on the surface of the carbon matrix, and a lithium / carbon composite layer is formed on the surface of the lithium metal particles. The composite lithium metal negative electrode material can effectively improve the growth of lithium dendrites and slow down the volume expansion of the lithium negative electrode, thereby having good lithium storage performance and excellent cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a composite lithium metal negative electrode material and a preparation method and application thereof. Background Art

[0002] The cruising range of a vehicle is one of the key indicators that determine the core competitiveness of new energy vehicles. The development of high-energy-density power batteries is the fundamental way to improve the cruising range of the vehicle. The mass-produced nickel-cobalt-manganese 811 positive electrode matched with a graphite negative electrode power cell has an energy density of more than 280Wh / kg. The energy density of the battery cell needs to be steadily improved through the improvement of positive and negative electrode materials, as well as the matching and upgrading of other materials.

[0003] Although the lithium-ion battery system based on graphite anode has achieved great success, its relatively low theoretical energy density limits its further application as the anode material of the next generation of power batteries. Compared with the graphite anode, metallic lithium has an extremely high specific capacity (3860mAh*g -1 ) and extremely low reduction potential (-3.040 V relative to standard hydrogen electrode), thus promoting the potential application of metal lithium batteries. However, the widespread application of metal lithium electrodes is severely hindered by multiple challenges, such as the uncontrolled generation of dendritic and powdery lithium and the large volume expansion of the lithium negative electrode during the deposition and removal process. These inherent shortcomings of the metal lithium negative electrode significantly reduce the cycle life of the battery and even lead to catastrophic safety issues.

[0004] Carbon materials are often used as carriers of lithium metal due to their unique and controllable properties. First, carbon materials themselves have good chemical and electrochemical stability and sufficient mechanical strength. Secondly, the conductivity, pore structure, surface area and lithium-philic sites of carbon-based carriers can be adjusted independently or in a coordinated manner according to actual requirements. Among them, the conductivity and surface area can improve the current density of the electrode body and inhibit the formation of lithium dendrites. The rich pore structure can provide sufficient space for lithium metal to limit or eliminate volume changes before and after cycling. Carbon carriers with lithium-philic sites can adjust the uniformity of the lithium ion electric field and promote the uniform deposition of lithium metal. Existing improvement methods mainly focus on adding physical or chemical protective films to the surface of the lithium negative electrode and improving the structure of the lithium negative electrode matrix. Among them, the physical protective film method is simple and easy, such as the carbon microsphere protective film obtained by using a metal organic framework (CN109904391A). However, this approach has high requirements on the ionic / electronic conductivity and mechanical strength of the membrane. The regulation of local lithium deposition is difficult to achieve through a simple barrier method, and the use of non-in-situ synthesis methods is not easy to scale up production. In the large-scale preparation process, it is easy to have poor material consistency or uncontrollable uniformity. Summary of the invention

[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a composite lithium metal negative electrode material and a preparation method and application thereof. The composite lithium metal negative electrode material can effectively improve the growth of lithium dendrites, slow down the volume expansion of the lithium negative electrode, and thus has good lithium storage performance and excellent cycle stability.

[0006] In one aspect of the present invention, the present invention provides a composite lithium metal negative electrode material. According to an embodiment of the present invention, the composite lithium metal negative electrode material comprises a carbon matrix and lithium metal particles, wherein the lithium metal particles are distributed inside and / or on the surface of the carbon matrix, and a lithium / carbon composite layer is formed on the surface of the lithium metal particles.

[0007] According to the composite lithium metal negative electrode material including a carbon matrix and lithium metal particles according to an embodiment of the present invention, the lithium metal particles are distributed inside and / or on the surface of the carbon matrix. By dispersing the lithium metal particles in the carbon matrix, the volume expansion of lithium during the charge and discharge process can be reduced due to the inhibitory effect of the carbon matrix. At the same time, a lithium / carbon composite layer is formed on the surface of the lithium metal particles. The lithium / carbon composite layer can reduce the effective current density and make the ion flux uniform, that is, the lithium / carbon composite layer on the surface of the lithium metal particles can make the potential distribution around the lithium metal particles more uniform, and the lithium ions can be uniformly transmitted, thereby inhibiting the generation of lithium dendrites and improving the cycle life. Therefore, the composite lithium metal negative electrode material can effectively improve the growth of lithium dendrites, slow down the volume expansion of the lithium negative electrode, and thus has good lithium storage performance and excellent cycle stability.

[0008] In addition, the composite lithium metal negative electrode material according to the above embodiment of the present invention may also have the following technical features:

[0009] In some embodiments of the present invention, the particle size of the carbon matrix is ​​1-50 μm, and the particle size of the lithium metal particles is 10-300 nm. Thus, the composite lithium metal negative electrode material can have good lithium storage performance and excellent cycle stability.

[0010] In some embodiments of the present invention, the thickness of the lithium / carbon composite layer is 5-30 nm. Thus, the composite lithium metal negative electrode material can have good lithium storage performance and excellent cycle stability.

[0011] In some embodiments of the present invention, the mass proportion of the lithium metal particles is 30-80%. Thus, the composite lithium metal negative electrode material can have good lithium storage performance and excellent cycle stability.

[0012] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned composite lithium metal negative electrode material. According to an embodiment of the present invention, the method comprises:

[0013] (1) melting metallic lithium at high temperature to obtain molten lithium;

[0014] (2) Under the protection of an inert atmosphere, the precursor organic carbon source and the molten lithium are sprayed into a high-temperature furnace simultaneously for mixed carbonization to obtain a composite lithium metal negative electrode material.

[0015] The method comprises spraying a precursor organic carbon source and molten lithium into a high-temperature furnace respectively and simultaneously under the protection of an inert atmosphere, wherein the liquid phase precursor organic carbon source and the molten metallic lithium are mixed in the high-temperature furnace after spraying, and the liquid phase precursor organic carbon source is carbonized at high temperature to form a spherical or blocky carbon matrix, and the molten metallic lithium microsphere particles are dispersed inside and / or on the surface of the carbon matrix, and a lithium single substance is formed after cooling. The volume expansion of lithium during the charge and discharge process can be reduced by the inhibitory effect of the carbon matrix. On the other hand, due to the differences in reaction activity, temperature, etc. at the interface between the lithium metal and the carbon layer, the carbon close to the lithium metal has a higher crystallinity and a denser structure, and a small amount of metallic lithium is doped in the dense carbon structure. Therefore, a dense lithium / carbon composite layer is formed on the surface of the lithium metal particle. The lithium / carbon composite layer on the surface of the lithium metal particle can make the potential distribution around the lithium metal particle more uniform, and lithium ions can be evenly transmitted, thereby inhibiting the generation of lithium dendrites and improving the cycle life. Therefore, this method can be used to prepare a composite lithium metal negative electrode material that can effectively improve the growth of lithium dendrites and slow down the volume expansion of the lithium negative electrode. This method is an in-situ composite preparation method with strong controllability and repeatability, and is suitable for batch preparation.

[0016] In addition, the method for preparing a composite lithium metal negative electrode material according to the above embodiment of the present invention may also have the following technical features:

[0017] In some embodiments of the present invention, in step (2), the precursor organic carbon source includes an organic small molecule compound. Thus, the composite lithium metal negative electrode material can have good lithium storage performance and excellent cycle stability.

[0018] In some embodiments of the present invention, the organic small molecule compound includes at least one of benzene, toluene, p-xylene, m-xylene, phenol, naphthalene, anthracene, phenanthrene, pyrene, styrene, pyridine and nitrogen-methylpyrrolidone, preferably pyridine and nitrogen-methylpyrrolidone. Thus, the composite lithium metal negative electrode material can have good lithium storage performance and excellent cycle stability.

[0019] In some embodiments of the present invention, in step (2), the carbonization temperature is 500-1330° C., and the carbonization time is 1-8 hours. Thus, the composite lithium metal negative electrode material can have good lithium storage performance and excellent cycle stability.

[0020] In some embodiments of the present invention, in step (2), the spraying method includes at least one of spraying, evaporation, sputtering, electroplating, chemical replacement, liquid phase chemical deposition and vapor phase chemical deposition.

[0021] In a third aspect of the present invention, a lithium battery is provided. According to an embodiment of the present invention, the lithium battery comprises a positive electrode and a negative electrode, and the negative electrode adopts the composite lithium metal negative electrode material or the composite lithium metal negative electrode material prepared by the above method. As a result, the lithium battery has high capacity, high rate performance and good cycle stability.

[0022] In a fourth aspect of the present invention, the present invention provides a vehicle. According to an embodiment of the present invention, the vehicle includes the above-mentioned lithium battery. Thus, the vehicle has higher safety performance and longer service life.

[0023] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0025] Figure 1 is a scanning electron microscope image of a composite lithium metal negative electrode material of an embodiment of the present invention;

[0026] Figure 2 is a scanning electron microscope image of a composite lithium metal negative electrode material of an embodiment of the present invention;

[0027] Figure 3 is a transmission electron microscope image of a composite lithium metal negative electrode material of an embodiment of the present invention;

[0028] Figure 4 is a transmission electron microscope image of a composite lithium metal negative electrode material of an embodiment of the present invention;

[0029] Figure 5 It is a cycle curve diagram of a symmetrical battery composed of the composite lithium metal negative electrode materials of Examples 1-3 of the present invention and the negative electrode materials of Comparative Examples 1-3 at 0.1C. DETAILED DESCRIPTION

[0030] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but are not to be construed as limiting the present invention.

[0031] In one aspect of the present invention, the present invention provides a composite lithium metal negative electrode material. According to an embodiment of the present invention, reference Figure 1-2 The composite lithium metal negative electrode material includes a carbon matrix 100 and lithium metal particles 200.

[0032] According to an embodiment of the present invention, referring to Figure 3-4 , lithium metal particles 200 are distributed inside and / or on the surface of the carbon matrix 100. By dispersing the lithium metal particles 200 in the carbon matrix 100, the volume expansion of lithium during the charging and discharging process can be reduced due to the inhibitory effect of the carbon matrix 100. Further, the particle size of the carbon matrix 100 is 1-50μm, and the particle size of the lithium metal particles is 10-300nm. The inventors found that if the particle size of the carbon matrix 100 is too large, it is not conducive to the rapid transmission of lithium ions in the carbon matrix; if the particle size of the lithium metal particles is too large, the volume expansion during the charging and discharging process will accelerate the pulverization of lithium metal particles, which is not conducive to structural maintenance. Therefore, the present application adopts a composite lithium metal negative electrode material including a carbon matrix 100 with a particle size of 1-50μm and lithium metal particles 200 with a particle size of 10-300nm, which has good lithium storage performance and excellent cycle stability.

[0033] According to an embodiment of the present invention, the mass proportion of lithium metal particles in the composite lithium metal negative electrode material is 30-80%. The inventors found that if the mass proportion of lithium metal particles is too large, the corresponding content of the carbon matrix is ​​too low, and the matrix support cannot be played, resulting in an unstable material structure and easy breakage, and the volume expansion of lithium metal is large, resulting in poor cycle performance; if the mass proportion of lithium metal particles is too small, the advantage of the high capacity of lithium metal active substances cannot be fully utilized. Therefore, the present application adopts a composite lithium metal negative electrode material in which the mass proportion of lithium metal particles is 30-80%, which has good lithium storage performance and excellent cycle stability.

[0034] According to an embodiment of the present invention, referring to Figure 4 , a lithium / carbon composite layer 300 is formed on the surface 200 of the lithium metal particle. The inventors found that the lithium / carbon composite layer 300 can reduce the effective current density and make the ion flux uniform, that is, the lithium / carbon composite layer 300 on the surface of the lithium metal particle 200 can make the potential distribution around the lithium metal particle 200 more uniform, and the lithium ions can be evenly transmitted, thereby inhibiting the generation of lithium dendrites and improving the cycle life. As a result, the composite lithium metal negative electrode material can effectively improve the growth of lithium dendrites, slow down the volume expansion of the lithium negative electrode, and thus have good lithium storage performance and excellent cycle stability. Furthermore, the thickness of the lithium / carbon composite layer 300 is 5-30nm. The inventors found that if the thickness of the lithium / carbon composite layer 300 is too small, the composite layer cannot play the role of inhibiting the expansion of lithium metal; if the thickness of the lithium / carbon composite layer 300 is too large, the proportion of active lithium metal components is small and the capacity of lithium metal is affected. Therefore, the present application adopts a lithium / carbon composite layer 300 with a thickness of 5-30 nm, and the composite lithium metal negative electrode material has good lithium storage performance and excellent cycle stability.

[0035] According to an embodiment of the present invention, in another aspect of the present invention, the present invention provides a method for preparing the above-mentioned composite lithium metal negative electrode material. According to an embodiment of the present invention, the method comprises:

[0036] S100: Melting Lithium Metal at High Temperature

[0037] In this step, the metallic lithium is melted at a high temperature to obtain molten lithium. It will be appreciated by those skilled in the art that the temperature for melting the metallic lithium is not limited, as long as the metallic lithium can be melted.

[0038] S200: Under the protection of inert atmosphere, the precursor organic carbon source and molten lithium are sprayed into a high temperature furnace for mixed carbonization.

[0039] In this step, the precursor organic carbon source and molten lithium are sprayed into a high-temperature furnace respectively and simultaneously under the protection of an inert atmosphere, wherein the liquid phase precursor organic carbon source and the molten metallic lithium are mixed in the high-temperature furnace after spraying, and the liquid phase precursor organic carbon source is carbonized at high temperature to form a spherical or blocky carbon matrix, and the molten metallic lithium microsphere particles are dispersed inside and / or on the surface of the carbon matrix, and lithium single substance is formed after cooling. The volume expansion of lithium during the charge and discharge process can be reduced by the inhibitory effect of the carbon matrix; on the other hand, due to the differences in reaction activity, temperature, etc. at the interface between the lithium metal and the carbon layer, the carbon close to the lithium metal has a higher crystallinity and a denser structure, and a small amount of metallic lithium is doped in the dense carbon structure. Therefore, a dense lithium / carbon composite layer is formed on the surface of the lithium metal particle, and the lithium / carbon composite layer on the surface of the lithium metal particle can make the potential distribution around the lithium metal particle more uniform, and lithium ions can be evenly transmitted, thereby inhibiting the generation of lithium dendrites and improving the cycle life. It should be noted that the spraying method is a conventional method in the field, and those skilled in the art can select it according to actual conditions. For example, the spraying method includes at least one of spraying, evaporation, sputtering, electroplating, chemical replacement, liquid phase chemical deposition and vapor phase chemical deposition.

[0040] According to an embodiment of the present invention, the precursor organic carbon source includes an organic small molecule compound. The inventors have found that the organic small molecule compound as a precursor organic carbon source is conducive to gas phase nucleation during the spraying and carbonization process, forming more uniform carbon microsphere particles with smaller particle size, good dispersibility, and not easy to agglomerate. However, if the organic molecules are too large, the reaction mechanism may be gas phase to liquid phase nucleation, and the particles are large, which is not conducive to the uniform attachment and dispersion of lithium metal. Therefore, the present application uses an organic small molecule compound as a precursor organic carbon source to prepare a composite lithium metal negative electrode material with good lithium storage performance and excellent cycle stability. It can be understood by those skilled in the art that organic small molecule compounds are conventional compounds in the art, and those skilled in the art can select them according to actual conditions. For example, organic small molecule compounds include but are not limited to at least one of benzene, toluene, p-xylene, m-xylene, phenol, naphthalene, anthracene, phenanthrene, pyrene, styrene, pyridine and nitrogen methyl pyrrolidone. The inventors have found that if the organic small molecule compound contains polar functional groups such as oxygen and nitrogen, the polar functional groups can serve as affinity sites to induce homogenized lithium ion distribution, increase the nucleation sites of lithium, and facilitate more uniform deposition of lithium, thereby improving the electrochemical performance of the negative electrode material. Therefore, the organic small molecule compound is preferably pyridine or nitrogen-methylpyrrolidone.

[0041] According to an embodiment of the present invention, the carbonization temperature is 500-1330°C, and the carbonization time is 1-8h. The inventors found that if the carbonization temperature is too high and the carbonization time is too long, on the one hand, lithium metal melt agglomeration is likely to occur, and on the other hand, the graphitization degree of the carbon matrix is ​​increased and the interlayer spacing of the carbon layer is reduced, which is not conducive to the rapid deintercalation of lithium ions; if the carbonization temperature is too low and the carbonization time is too short, the precursor carbonization is incomplete, the carbon matrix structure is unstable, and some unreacted functional groups may have side reactions during the charge and discharge process, resulting in irreversible capacity loss. Therefore, by adopting the carbonization temperature of 500-1330°C and the carbonization time of 1-8h in this application, a composite lithium metal negative electrode material with good lithium storage performance and excellent cycle stability can be prepared.

[0042] Therefore, this method can be used to prepare a composite lithium metal negative electrode material that can effectively improve the growth of lithium dendrites and slow down the volume expansion of the lithium negative electrode. This method is an in-situ composite preparation method with strong controllability and repeatability, and is suitable for batch preparation.

[0043] In the third aspect of the present invention, the present invention provides a lithium battery. According to an embodiment of the present invention, the lithium battery includes a positive electrode and a negative electrode, and the negative electrode adopts the above-mentioned composite lithium metal negative electrode material or the composite lithium metal negative electrode material prepared by the above-mentioned method. As a result, the lithium battery has high capacity, high rate performance and good cycle stability. It should be noted that the features and advantages described above for the composite lithium metal negative electrode material and its preparation method are also applicable to the lithium battery, which will not be repeated here.

[0044] In a fourth aspect of the present invention, a vehicle is provided. According to an embodiment of the present invention, the vehicle includes the above-mentioned lithium battery. As a result, the vehicle has higher safety performance and longer service life. It should be noted that the features and advantages described above for the lithium battery are also applicable to the vehicle and will not be described in detail here.

[0045] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0046] Example 1

[0047] (1) Solid lithium metal is heated to 300° C. to melt, and is sprayed simultaneously with a precursor carbon source benzene in a high-temperature furnace at 800° C. under the protection of an inert gas, and is kept warm for 2 hours for carbonization to form lithium metal particles dispersed in and / or on the surface of micron carbon spheres (carbon matrix). After cooling, the composite lithium metal negative electrode material is obtained by sieving through a 400-mesh sieve, wherein the mass proportion of lithium metal particles in the composite lithium metal negative electrode material is 50%.

[0048] (2) The above-mentioned composite lithium metal negative electrode material was observed by SEM and TEM, and it can be obtained that the particle size of the spherical carbon matrix is ​​1-5μm, the particle size of the lithium metal particles is 40-60nm, and the thickness of the lithium / carbon composite layer coated on the surface of the lithium metal particles is 10nm.

[0049] Example 2

[0050] (1) Solid lithium metal is heated to 450° C. to melt, and a precursor carbon source mixed with toluene and pyridine is sprayed simultaneously in a high-temperature furnace at 950° C. under the protection of an inert gas, and the mixture is kept warm for 1 hour for carbonization to form lithium metal particles dispersed in and / or on the surface of micron carbon spheres (carbon matrix). After cooling, the mixture is sieved through a 400-mesh sieve to obtain a composite lithium metal negative electrode material, wherein the mass proportion of lithium metal particles in the composite lithium metal negative electrode material is 40%.

[0051] (2) The above-mentioned composite lithium metal negative electrode material was observed by SEM and TEM, and it can be obtained that the particle size of the spherical carbon matrix is ​​5-10μm, the particle size of the lithium metal particles is 30-50nm, and the thickness of the lithium / carbon composite layer coated on the surface of the lithium metal particles is 5-7nm.

[0052] Example 3

[0053] (1) Solid lithium metal is heated to 300° C. to melt, and a precursor carbon source mixed with naphthalene and nitrogen methyl pyrrolidone is sprayed simultaneously in a high-temperature furnace at 1000° C. under the protection of an inert gas, and the mixture is kept warm for 1 hour for carbonization to form lithium metal particles dispersed in and / or on the surface of micron carbon spheres (carbon matrix). After cooling, the mixture is sieved through a 400-mesh sieve to obtain a composite lithium metal negative electrode material, wherein the mass proportion of lithium metal particles in the composite lithium metal negative electrode material is 30%.

[0054] (2) The above-mentioned composite lithium metal negative electrode material was observed by SEM and TEM, and it can be obtained that the particle size of the spherical carbon matrix is ​​10-30μm, the particle size of the lithium metal particles is 20-40nm, and the thickness of the lithium / carbon composite layer coated on the surface of the lithium metal particles is 5nm.

[0055] Comparative Example 1

[0056] Solid metal lithium is heated to 300°C to melt, and physically mixed with mesophase asphalt microspheres. After cooling, a bulk composite negative electrode material of lithium metal and mesophase asphalt is formed, and the mass fraction of metal lithium in the composite negative electrode material is 50%.

[0057] Comparative Example 2

[0058] Solid metal lithium is heated to 400°C to melt, and physically mixed with mesophase asphalt microspheres. After cooling, a bulk composite negative electrode material of lithium metal and mesophase asphalt is formed, and the mass fraction of metal lithium in the composite negative electrode material is 40%.

[0059] Comparative Example 3

[0060] Solid metal lithium is heated to 450°C to melt, and physically mixed with mesophase asphalt microspheres. After cooling, a bulk composite negative electrode material of lithium metal and mesophase asphalt is formed, and the mass fraction of metal lithium in the composite negative electrode material is 30%.

[0061] The electrochemical performance test method for the composite lithium metal negative electrode materials of Examples 1-3 and the negative electrode materials of Comparative Examples 1-3 is as follows:

[0062] Half-cell test method: In an inert atmosphere glove box, the composite lithium metal negative electrode materials of Examples 1-3 and the negative electrode materials of Comparative Examples 1-3 were used as positive electrodes, lithium sheets were used as negative electrodes, 1M LiPF6 was used as the electrolyte, and the solvent was EC:DEC:DMC=1:1:1, and assembled into 2032 button-type half-cells. Subsequently, the electrochemical performance test was carried out at 0.5 mA / cm 2 and 2mA / cm 2The constant current charge and discharge were performed at a fixed current density, and the discharge was performed for 1 hour (this process corresponds to lithium deposition). The charging voltage reached 1.0V (this process corresponds to lithium stripping). The lithium metal stripping / deposition efficiency (i.e., its coulombic efficiency) and cycle capacity retention rate were tested. The test voltage range was 0.01-1.0V. The test results are shown in Table 1.

[0063] Full battery test method: In an inert atmosphere glove box, the composite lithium metal negative electrode material of Example 1-3 and the negative electrode material of Comparative Example 1-3 are used as counter electrodes to assemble Li / C-Li / C symmetrical batteries, and a solution of 1M LiTFSI in DME:DOL=1:1 (volume ratio) is used as the electrolyte. The electrolyte contains 2wt% lithium nitrate as an additive. Each sample is assembled into 3 2032 button batteries for electrochemical testing to evaluate its long-cycle cycle performance. The test temperature is 25°C, the test voltage range is 0.01-1V, and the cycle test is 1C charge and discharge for 100 weeks. The test results are shown in Table 2. The cycle results of the symmetrical battery composed of the composite lithium metal negative electrode material of Example 1-3 and the negative electrode material of Comparative Example 1-3 at 0.1C are shown in Table 2. Figure 5 shown.

[0064] Table 1

[0065]

[0066] It can be seen from Table 1 that the half-cells prepared from the composite lithium metal negative electrode materials of Examples 1-3 have a current density of 0.5 mA / cm 2 and 2mA / cm 2 The first coulombic efficiency and 500 cycle capacity retention rate are better than those of the negative electrode materials in comparative examples 1-3, indicating that the composite lithium metal negative electrode material of the present application can effectively improve the cycle stability and rate performance, especially when the lithium content is high, the protective effect of the carbon matrix is ​​more prominent, and the electrochemical performance of the composite lithium metal material in the embodiment is better than that of the block material in the comparative example.

[0067] Table 2

[0068]

[0069] As can be seen from Table 2, from Examples 1 to 3, the higher the lithium metal content, the higher the discharge capacity of the material, and the same trend is found in the comparative examples. However, the composite lithium metal negative electrodes with the same lithium metal content have better electrochemical performance than the bulk materials in the corresponding examples. The first efficiency of Examples 1-3 is high, all above 85%, and the cycle retention rate of 100 weeks is above 90%; while the attenuation of Comparative Examples 1-3 is more serious, and the cycle retention rate of 100 weeks is less than 50%.

[0070] from Figure 5It can be seen more clearly that the cycle curves of Examples 1-3 are smoother, while the cycle curves of Comparative Examples 1-3 decay faster. This is mainly because the special composite structure in the embodiments is beneficial to inhibiting the cycle attenuation caused by the volume expansion of lithium metal, and inhibiting the generation of lithium dendrites to improve the cycle life.

[0071] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0072] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a composite lithium metal negative electrode material, characterized in that: include: (1) Melting metallic lithium at high temperature to obtain molten lithium; (2) spraying the precursor organic carbon source and the molten lithium into a high-temperature furnace for mixed carbonization under the protection of an inert atmosphere to obtain a composite lithium metal negative electrode material; The composite lithium metal negative electrode material comprises a carbon matrix and lithium metal particles. The lithium metal particles are distributed inside and / or on the surface of the carbon matrix, and a lithium / carbon composite layer is formed on the surface of the lithium metal particles.

2. The method according to claim 1, characterized in that In step (2), the precursor organic carbon source includes an organic small molecule compound.

3. The method according to claim 2, characterized in that The organic small molecule compound includes at least one of benzene, toluene, p-xylene, m-xylene, phenol, naphthalene, anthracene, phenanthrene, pyrene, styrene, pyridine and nitrogen methyl pyrrolidone.

4. The method according to claim 2, characterized in that: The organic small molecule compound is pyridine or nitrogen methyl pyrrolidone.

5. The method according to claim 1, characterized in that In step (2), the carbonization temperature is 500-1330° C., and the carbonization time is 1-8 hours.

6. The method according to claim 1, characterized in that In step (2), the spraying method includes at least one of spraying, evaporation, sputtering, and vapor phase chemical deposition.

7. A composite lithium metal negative electrode material prepared by the method according to any one of claims 1 to 6, characterized in that: The invention comprises a carbon matrix and lithium metal particles. The lithium metal particles are distributed inside and / or on the surface of the carbon matrix, and a lithium / carbon composite layer is formed on the surface of the lithium metal particles.

8. The composite lithium metal negative electrode material according to claim 7, characterized in that: The particle size of the carbon matrix is ​​1-50 μm, and the particle size of the lithium metal particles is 10-300 nm.

9. The composite lithium metal negative electrode material according to claim 8, characterized in that The thickness of the lithium / carbon composite layer is 5-30 nm.

10. The composite lithium metal negative electrode material according to claim 7, characterized in that: The mass proportion of the lithium metal particles is 30-80%.

11. A lithium battery, characterized in that: It comprises a positive electrode and a negative electrode, wherein the negative electrode is a composite lithium metal negative electrode material as described in any one of claims 7 to 10 or a composite lithium metal negative electrode material prepared by the method as described in any one of claims 1 to 6.

12. A vehicle, characterized in that: The vehicle includes the lithium battery of claim 11.