A cross-linking agent and preparation method thereof, and photoresist

By using a new cross-linking agent in the photoresist, the problem of uneven chemical reactions caused by light source exposure is solved, graphic morphology defects are improved, more vertical line edges and larger windows are achieved, while environmental pollution is reduced and risk of deformation of the photoresist layer.

CN115947648BActive Publication Date: 2024-10-18BEIJING RED AVENUE INNOVA +3
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211695370.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-10-18
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

When the photoresist is exposed to a light source, the chemical reaction is uneven due to uneven light intensity distribution, which leads to defects in the pattern morphology, such as the bottom of the groove is not developed cleanly or the side walls of the three-dimensional pattern are not vertical enough.

Method used

Design a new cross-linker with a structure that promotes a more uniform cross-linking reaction between resin and cross-linker in the photoresist, reduces local molecular weight differences, includes specific hydroxyl OH groups to improve dissolution rate and contrast, and It is prepared through an acidic catalytic reaction to ensure that the cross-linking agent does not release a large amount of low-boiling point alcohols during the cross-linking process, thereby reducing environmental pollution and morphological effects.

Benefits of technology

It achieves more vertical edges of photoresist pattern lines, larger windows, reduces morphological defects, reduces the risk of photoresist layer deformation and cracking, and improves the contrast between exposed and non-exposed areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115947648B_ABST
    Figure CN115947648B_ABST
Patent Text Reader

Abstract

The present application provides a cross-linking agent and a preparation method thereof, and a photoresist, belonging to the field of photolithography technology. The photoresist includes a solute and a first solvent, wherein the solute includes 70wt% to 95wt% of an alkali-soluble resin, 1wt% to 30wt% of a photoacid generator, 0.1wt% to 15wt% of an acid quencher, and 5wt% to 20wt% of the above-mentioned cross-linking agent, and the mass of the first solvent is 1 to 10 times the mass of the alkali-soluble resin. The cross-linking agent of the present application can be added to the photoresist, and the cross-linking reaction of the matrix resin of the photoresist is made more uniform, reducing or avoiding morphological defects caused by excessive local molecular weight, and the edges of the obtained graphic lines are more vertical, and the window is larger.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photolithography technology, and in particular to a cross-linking agent and a preparation method thereof, and a photoresist. Background Art

[0002] Photoresist is one of the key materials for fine pattern processing in microelectronics technology. Especially in recent years, the development of large-scale and ultra-large-scale integrated circuits has greatly promoted the research, development and application of photoresist.

[0003] Negative photoresist based on the principle of photochemical amplification contains photoacid generator and crosslinking agent. After exposure, acid is released. Photoacid generator can catalyze the interaction between crosslinking agent and resin to cause crosslinking. The crosslinked resin is different from the resin in the unexposed area and becomes insoluble in the developer, leaving a pattern opposite to the mask on the substrate material. The speed of crosslinking reaction between resin and crosslinking agent and whether the crosslinking reaction is uniform have a decisive influence on the performance of photoresist.

[0004] Photoresists are designed for exposure wavelengths. G-line 436nm, I-line 365nm, KrF 248nm and ArF 193nm are the mainstream exposure light source wavelengths in the industry. When the light source is exposed, the light intensity is distributed in the film in a longitudinal gradient, so the photon concentration is also longitudinally non-uniform, which leads to longitudinal non-uniformity in the chemical reaction. This means that the cross-linking reaction between the resin and the cross-linking agent at different positions in the pattern is also different. If the local molecular weight difference is too large due to the different degree of cross-linking reaction, the produced pattern morphology is very likely to have defects. Summary of the invention

[0005] The present application provides a cross-linking agent and a preparation method thereof, and a photoresist, which can improve the morphological defects of the obtained graphics.

[0006] The embodiment of the present application is implemented as follows:

[0007] In the first aspect, the present application provides a cross-linking agent, the structural formula of which is as follows:

[0008]

[0009] Wherein, R1, R2, R3, R4 and R5 are each independently selected from H, OH,

[0010] or -R 12 -OR 13 .

[0011] R6 is selected from C 1~10 alkyl.

[0012] R7, R8 and R9 are each independently selected from H, C 1~6 Saturated or unsaturated alkyl, C 1~6 Saturated or unsaturated cycloalkyl, -OR 15 or

[0013] R 10 Selected from C 1~5 alkyl.

[0014] R 11 Selected from C 1~20 alkyl.

[0015] R 12 Selected from C 1~5 alkyl.

[0016] R 13 Selected from C 1~20 alkyl.

[0017] R 14 Selected from C 1~20 alkyl.

[0018] R 15 Selected from C 1~20 alkyl.

[0019] R 16 , R 17 , R 18 , R 19 and R 20 Each independently selected from H, OH,

[0020] or -R 12 -OR 13 .

[0021] R1, R2, R3, R4, R5, R 16 , R 17 , R 18 , R 19 and R 20 Any at least two of the above are selected from at least one of the first group and the second group.

[0022] The structural formula of the first group is

[0023] The structural formula of the second group is -R 12 -OR 13 , and R 13 Not for H.

[0024] In the above technical scheme, the crosslinking agent of the present application can be added to the photoresist to make the crosslinking reaction of the matrix resin of the photoresist more uniform, reduce or avoid morphological defects caused by excessive local molecular weight, and obtain a more vertical edge of the graphic lines and a larger window.

[0025] In combination with the first aspect, in a first possible example of the first aspect of the present application, the above R 13 Selected from C 8~14 Alkyl, R 15 Selected from C 8~14 alkyl.

[0026] In the above examples, the cross-linking agent of the present application will not release a large amount of low-boiling alcohols during the cross-linking reaction, that is, the cross-linking agent will not cause pollution to the environment, and is a green and environmentally friendly cross-linking agent. At the same time, the volatilization of low-boiling alcohols will not have an adverse effect on the morphology of the photoresist. In addition, the small molecule alcohols that are difficult to volatilize produced by the cross-linking agent during the cross-linking reaction can alleviate the stress problem between the substrate and the photoresist caused by the hard film, and reduce the risk of deformation and cracking of the photoresist layer.

[0027] In combination with the first aspect, in a second possible example of the first aspect of the present application, the above R1, R2, R3, R4, R5, R 16 , R 17 , R 18 , R 19 and R 20 Any 2 to 4 of them are selected from at least one of the first group and the second group.

[0028] In combination with the first aspect, in a third possible example of the first aspect of the present application, any 1 to 2 of the above R1, R2, R3, R4 and R5 are selected from at least one of the first group and the second group, and R 16 , R 17 , R 18 , R 19 and R 20 Any 1 to 2 of them are selected from at least one of the first group and the second group.

[0029] In combination with the first aspect, in a fourth possible example of the first aspect of the present application, the above R1, R2, R3, R4, R5, R 16 , R 17 , R 18 , R 19 and R 20 Any 1 to 5 of them are selected from OH.

[0030] In the above example, appropriate hydroxyl groups OH in the cross-linking agent can increase the dissolution rate of the photoresist, which is beneficial to improving the contrast between the exposed area and the non-exposed area, while reducing the risk of residual photoresist in the non-exposed area.

[0031] In combination with the first aspect, in a fifth possible example of the first aspect of the present application, the R 10 Selected from CH2.

[0032] In combination with the first aspect, in a sixth possible example of the first aspect of the present application, the above R9 is selected from

[0033] In the second aspect, the present application provides an example of a method for preparing the cross-linking agent of the above embodiment, which comprises: subjecting a hydroxyalkylphenol compound and a reactant to an acidic catalytic reaction to obtain an intermediate, and then neutralizing the intermediate.

[0034] The structural formula of hydroxyalkylphenol compounds is as follows.

[0035]

[0036] Among them, R 21 , R 22 , R 23 , R 24 and R 25 Each independently selected from H, OH or -R 12 -OH.

[0037] R 12 Selected from C 1~10 alkyl.

[0038] R 26 Selected from C 1~10 alkyl.

[0039] R 27 , R 28 and R 29 Each independently selected from H, C 1~6 Saturated or unsaturated alkyl, C 1~6 Saturated or unsaturated cycloalkyl or

[0040] R 30 , R 31 , R 32 , R 33 and R 34 Each independently selected from H, OH or -R 35 -OH.

[0041] R 35 Selected from C 1~10 alkyl.

[0042] R21 , R 22 , R 23 , R 24 , R 25 , R 30 , R 31 , R 32 , R 33 and R 34 Any at least two of the three groups are selected from at least one of the third group and the fourth group.

[0043] The structural formula of the third group is -R 12 -OH.

[0044] The structural formula of the fourth group is -R 35 -OH.

[0045] The reactants include at least one of an alkylphenol compound and an alcohol compound.

[0046] The structural formula of alkylphenol compounds is as follows:

[0047]

[0048] Among them, R 36 , R 37 Each independently selected from H or -R 38 .

[0049] R 38 Selected from C 1-20 Saturated or unsaturated alkyl.

[0050] R 36 , R 37 Any at least one selected from -R 38 .

[0051] The structural formula of alcohol compounds is as follows:

[0052]

[0053] n is 0 to 19.

[0054] In the above technical solution, the preparation method of the cross-linking agent of the present application has a simple process and is easy to realize industrial production.

[0055] In combination with the second aspect, in a first possible example of the second aspect of the present application, the acid catalytic reaction temperature is 50° C. to 150° C., and the reaction time is 0.4 h to 12 h.

[0056] Optionally, the molar ratio of the hydroxyalkylphenol compound to the reactant is 1:2 to 1:4.

[0057] In the above examples, in the preparation method of the cross-linking agent of the present application, the reaction conditions and temperature are safe and reliable.

[0058] In the third aspect, the present application provides an example of a photoresist, which includes: a solute and a first solvent, wherein the solute includes 70wt% to 95wt% of an alkali-soluble resin, 1wt% to 30wt% of a photoacid generator, 5wt% to 20wt% of the cross-linking agent of the above-mentioned embodiment and 0.1wt% to 15wt% of an acid quencher, and the mass of the first solvent is 1 to 10 times the mass of the alkali-soluble resin.

[0059] Optionally, the alkali-soluble resin includes any one or more of poly(p-hydroxystyrene) resin, polystyrene resin, poly(p-hydroxystyrene) resin and linear phenolic resin.

[0060] Optionally, the photoacid generator includes any one or more of iodonium salts, sulfonium salts and heterocyclic acid generators.

[0061] Optionally, the acid quencher comprises a basic organic substance.

[0062] Optionally, the alkaline organic substance includes tertiary ammonium and / or quaternary ammonium compounds.

[0063] Optionally, the first solvent includes any one or more of 1,2-propylene glycol methyl ether acetate, ethyl lactate and ethyl acetate.

[0064] In the above technical solution, the photoresist of the present application has fewer or no morphological defects during use, the edges of the graphic lines are more vertical, and the windows are larger. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0066] Figure 1 A schematic diagram of a pattern having a first defect after photoresist development;

[0067] Figure 2 is a schematic diagram of a second defect of a pattern after photoresist development;

[0068] Figure 3 It is a schematic diagram of a pattern formed after the photoresist is developed in Example 1 of the present application at a focal length of -0.3 to 0.3;

[0069] Figure 4It is a schematic diagram of a pattern formed after the photoresist is developed in Example 2 of the present application at a focal length of -0.3 to 0.3;

[0070] Figure 5 It is a schematic diagram of a pattern formed after the photoresist is developed in Example 3 of the present application at a focal length of -0.3 to 0.3;

[0071] Figure 6 It is a schematic diagram of a pattern formed after the photoresist is developed in Example 4 of the present application at a focal length of -0.3 to 0.3;

[0072] Figure 7 It is a schematic diagram of a pattern formed after the photoresist is developed in Example 5 of the present application at a focal length of -0.3 to 0.3;

[0073] Figure 8 It is a schematic diagram of a pattern formed after the photoresist is developed in Example 6 of the present application at a focal length of -0.3 to 0.3;

[0074] Fig. 9 It is a schematic diagram of a pattern formed after the photoresist is developed in Example 7 of the present application at a focal length of -0.3 to 0.3;

[0075] Fig.10 This is a schematic diagram of a pattern formed after the photoresist in Comparative Example 1 of the present application is developed at a focal length of -0.3 to 0.3;

[0076] Fig.11 This is a schematic diagram of a pattern formed after the photoresist of Example 1 of the present application is developed at a film thickness of 20 μm;

[0077] Fig.12 This is a schematic diagram of a pattern formed after the photoresist of comparative example 1 of the present application is developed at a film thickness of 20 μm. DETAILED DESCRIPTION

[0078] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0079] Photoresist, also known as photoresist, refers to a thin film material whose solubility changes when exposed to ultraviolet light, electron beam, ion beam, X-ray, etc. It can be widely used in fine pattern processing, such as the manufacture of integrated circuits, flat panel displays and semiconductor discrete devices.

[0080] The inventors of the present invention noticed that when the light source is exposed, the distribution of light intensity in the film is distributed in a longitudinal gradient, so the photon concentration is also longitudinally non-uniform, which leads to longitudinal non-uniformity in the chemical reaction induced. This means that there are differences in the cross-linking reaction between the resin and the cross-linking agent at different positions in the pattern. If the local molecular weight difference is too large due to the different degrees of cross-linking reaction, the produced pattern morphology is very likely to have defects. For example, the bottom or top of the groove is not developed cleanly, or the side wall of the three-dimensional pattern is not vertical enough, and the bottom is prone to tailing. Figure 1 and 2 As shown, Figure 1 The morphological defect shown is that the 200nm space is not completely opened and there is adhesion. Figure 2 The morphological defect shown is that there is a tail at the bottom of the 200nm space morphology.

[0081] In order to improve the defect problem of photoresist pattern morphology, the applicant has found that the pattern morphology can be improved by increasing the uniformity of the cross-linking reaction of the resin at different positions in the photoresist.

[0082] Based on the above considerations, in order to improve the graphic morphology by improving the uniformity of the resin cross-linking reaction at different positions in the photoresist, the inventors have designed a cross-linking agent after in-depth research, which can be added to the photoresist and make the cross-linking reaction of the matrix resin of the photoresist more uniform, thereby reducing or avoiding morphological defects caused by excessive local molecular weight, and the edges of the obtained graphic lines are more vertical and the windows are larger.

[0083] The present application provides a cross-linking agent, the structural formula of which is as follows:

[0084]

[0085] Wherein, R1, R2, R3, R4 and R5 are each independently selected from H, OH,

[0086] or -R 12 -OR 13 .

[0087] R6 is selected from C 1~10 alkyl.

[0088] R7, R8 and R9 are each independently selected from H, C 1~6 Saturated or unsaturated alkyl, C 1~6 Saturated or unsaturated cycloalkyl, -OR 15 or

[0089] R 10 Selected from C 1~5 alkyl.

[0090] R 11 Selected from C 1~20 alkyl.

[0091] R 12 Selected from C 1~5 alkyl.

[0092] R 13 Selected from C 1~20 alkyl.

[0093] R 14 Selected from C 1~20 alkyl.

[0094] R 15 Selected from C 1~20 alkyl.

[0095] R 16 , R 17 , R 18 , R 19 and R 20 Each independently selected from H, OH,

[0096] or -R 12 -OR 13 .

[0097] R1, R2, R3, R4, R5, R 16 , R 17 , R 18 , R 19 and R 20 Any at least two of the above are selected from at least one of the first group and the second group.

[0098] The structural formula of the first group is

[0099] The structural formula of the second group is -R 12 -OR 13 , and R 13 Not for H.

[0100] As an example, R1, R2, R3, R4, R5, R 16 , R 17 , R 18 , R 19 and R 20 At least two of any two may be R1 and R2, R1 and R3, R1 and R4, R1 and R5, R1 and R 16 , R1 and R 17 , R1 and R 18 , R1 and R 19 , R1 and R 20, R2 and R3, R2 and R4, R2 and R5, R2 and R 16 , R2 and R 17 , R2 and R 18 , R2 and R 19 , R2 and R 20 , R3 and R4, R3 and R5, R3 and R 16 , R3 and R 17 , R3 and R 18 , R3 and R 19 , R3 and R 20 , R4 and R5, R4 and R 16 , R4 and R 17 , R4 and R 18 , R4 and R 19 , R4 and R 20 , R5 and R 16 , R5 and R 17 , R5 and R 18 , R5 and R 19 , R5 and R 20 , R 16 and R 17 , R 16 and R 18 , R 16 and R 19 , R 16 and R 20 , R 17 and R 18 , R 17 and R 19 , R 17 and R 20 , R 18 and R 19 , R 18 and R 20 , R 19 and R 20 , R1, R2 and R3, R1, R2 and R4, R2, R3 and R4, R1, R2, R3 and R4, R 16 , R 17 and R 18 , R1, R 17 and R 18 , R1, R5 and R 18 , R1, R2, R3 and R4, R2, R3, R4 and R5, R4, R5, R 16 and R 17 , R 16 , R 17 , R 18 and R 19 .

[0101] As an example, R1, R2, R3, R4, R5, R 16 , R 17 , R 18 , R 19 and R 20 At least two of any of can be both selected from the first group, or both selected from the second group, or partly selected from the first group and partly selected from the second group.

[0102] Optionally, R1, R2, R3, R4, R5, R 16 , R 17 , R 18 , R 19 and R 20 Any 2 to 4 of them are selected from at least one of the first group and the second group.

[0103] Optionally, any 1 to 2 of R1, R2, R3, R4 and R5 are selected from at least one of the first group and the second group, and R 16 , R 17 , R 18 , R 19 and R 20 Any 1 to 2 of them are selected from at least one of the first group and the second group.

[0104] Optionally, R1, R2, R3, R4, R5, R 16 , R 17 , R 18 , R 19 and R 20 Any 1 to 5 of them are selected from OH.

[0105] Appropriate hydroxyl groups OH in the cross-linking agent can increase the dissolution rate of the photoresist, which is beneficial to improving the contrast between the exposed area and the non-exposed area, while reducing the risk of photoresist residue in the non-exposed area.

[0106] Optionally, R 13 Selected from C 8~14 Alkyl, R 15 Selected from C 8~14 alkyl.

[0107] The cross-linking agent of the present application will not release a large amount of low-boiling alcohols during the cross-linking reaction, that is, the cross-linking agent will not cause pollution to the environment, and is a green and environmentally friendly cross-linking agent. At the same time, the volatilization of low-boiling alcohols will not have an adverse effect on the morphology of the photoresist. In addition, the small molecule alcohols that are difficult to volatilize produced by the cross-linking agent during the cross-linking reaction can alleviate the stress problem between the substrate and the photoresist caused by the hard film, and reduce the risk of deformation and cracking of the photoresist layer.

[0108] Optionally, R 10Selected from CH2.

[0109] Optionally, R9 is selected from

[0110] The present application also provides a method for preparing the cross-linking agent of the above embodiment, which comprises: adding reactants and a second solvent to a reaction bottle equipped with a stirring device, a thermometer and a reflux condenser, heating so that the reactants are completely dissolved in the second solvent to obtain a first mixture, adding an acidic catalyst to the first mixture to obtain a second mixture, slowly adding a hydroxyalkylphenol compound to the second mixture, controlling the reaction temperature to 50°C to 150°C, reacting under reflux for 0.4h to 12h to obtain an intermediate, neutralizing the intermediate and removing the second solvent by vacuuming under reduced pressure, discharging the material, and obtaining a cross-linking agent.

[0111] Wherein, the reactants include at least one of an alkylphenol compound and an alcohol compound.

[0112] It should be noted that the types of reactants and the amounts of the alkylphenol compound and the alcohol compound need to be determined according to the designed cross-linking agent.

[0113] The structural formula of alkylphenol compounds is as follows:

[0114]

[0115] Among them, R 36 , R 37 Each independently selected from H or -R 38 .

[0116] R 38 Selected from C 1-20 Saturated or unsaturated alkyl.

[0117] R 36 , R 37 Any at least one selected from -R 38 .

[0118] Optionally, the alkylphenol includes any one or more of cresol, xylenol, ethylphenol, propylphenol, tert-butylphenol, pentylphenol, heptylphenol, octylphenol, 2,4-di-tert-butylphenol, nonylphenol, decylphenol, dodecylphenol, tetradecylphenol, hexadecylphenol, octadecylphenol and cardanol.

[0119] The structural formula of alcohol compounds is as follows:

[0120]

[0121] n is 0 to 19.

[0122] Optionally, the alcohol compound includes any one or more of methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, decanol, dodecanol, tetradecanol, hexadecanol, octadecyl alcohol and eicosanol.

[0123] The second solvent includes any one or more of petroleum ether, chloroform, ethyl acetate, dichloromethane, toluene and xylene.

[0124] The mass ratio of the second solvent to the reactant is 0.2 to 4:1.

[0125] The acidic catalyst includes an organic acid catalyst and / or an inorganic acid catalyst.

[0126] Optionally, the organic acid catalyst includes any one or more of trifluoroacetic acid, trichloroacetic acid, dodecylbenzenesulfonic acid, benzenesulfonic acid, acetic acid and oxalic acid.

[0127] Optionally, the inorganic acid catalyst includes any one or more of hydrochloric acid, sulfuric acid, sulfurous acid, phosphoric acid and nitric acid.

[0128] The structural formula of hydroxyalkylphenol compounds is as follows:

[0129]

[0130] Among them, R 21 , R 22 , R 23 , R 24 and R 25 Each independently selected from H, OH or -R 12 -OH.

[0131] R 12 Selected from C 1~10 alkyl.

[0132] R 26 Selected from C 1~10 alkyl.

[0133] R 27 , R 28 and R 29 Each independently selected from H, C 1~6 Saturated or unsaturated alkyl, C 1~6 Saturated or unsaturated cycloalkyl or

[0134] R 30 , R 31 , R 32 , R 33 and R 34 Each independently selected from H, OH or -R 35 -OH.

[0135] R35 Selected from C 1~10 alkyl.

[0136] R 21 , R 22 , R 23 , R 24 , R 25 , R 30 , R 31 , R 32 , R 33 and R 34 Any at least two of the three groups are selected from at least one of the third group and the fourth group.

[0137] The structural formula of the third group is -R 12 -OH.

[0138] The structural formula of the fourth group is -R 35 -OH.

[0139] The molar ratio of the hydroxyalkylphenol compound to the reactant is 1:2 to 1:4.

[0140] As an example, the molar ratio of the hydroxyalkylphenol compound to the reactant may be 1:2, 1:2.5, 1:3, 1:3.5 or 1:4.

[0141] As an example, the reaction temperature may be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C.

[0142] As an example, the reaction time may be 0.4 h, 0.5 h, 0.8 h, 1 h, 2 h, 5 h, 8 h, 10 h or 12 h.

[0143] The temperature of the reduced pressure vacuum pumping is 110°C to 240°C.

[0144] As an example, the temperature of the reduced pressure vacuuming may be 110°C, 120°C, 150°C, 170°C, 190°C, 200°C, 210°C, 230°C or 240°C.

[0145] The time for reducing pressure and evacuating the vacuum is 20 minutes to 40 minutes.

[0146] As an example, the time for the reduced pressure evacuation may be 20 min, 30 min or 40 min.

[0147] The present application also provides a photoresist, which includes: a solute and a first solvent, wherein the solute includes 70wt% to 95wt% of an alkali-soluble resin, 1wt% to 30wt% of a photoacid generator, 5wt% to 20wt% of the cross-linking agent of the above-mentioned embodiment and 0.1wt% to 15wt% of an acid quencher, and the mass of the first solvent is 1 to 10 times the mass of the alkali-soluble resin.

[0148] Optionally, the alkali-soluble resin includes any one or more of poly(p-hydroxystyrene) resin, polystyrene resin, poly(p-hydroxystyrene) resin and linear phenolic resin.

[0149] Optionally, the photoacid generator includes any one or more of iodonium salts, sulfonium salts and heterocyclic acid generators.

[0150] Optionally, the acid quencher includes alkaline organic matter, wherein the alkaline organic matter includes tertiary ammonium and / or quaternary ammonium compounds.

[0151] Optionally, the acid quencher includes any one or more of triethanolamine, trioctylamine, tributylamine and trimethoxyethoxymethoxyethylamine.

[0152] Optionally, the first solvent includes any one or more of 1,2-propylene glycol methyl ether acetate, ethyl lactate and ethyl acetate.

[0153] The following is a further detailed description of a cross-linking agent and a preparation method thereof, and a photoresist of the present application in conjunction with embodiments.

[0154] Example 1

[0155] The embodiment of the present application provides a cross-linking agent and a preparation method thereof, and a photoresist, which comprises the following steps:

[0156] 1.0 mol of dodecylphenol, 1.0 mol of n-octanol and 100 mL of toluene were added to a 500 mL round-bottom flask equipped with a stirring device, a thermometer and a reflux condenser. The temperature was raised and stirred to completely dissolve the dodecylphenol and n-octanol in toluene to obtain a first mixture. 0.5 g of dodecylbenzenesulfonic acid was added to the first mixture to obtain a second mixture. 1.0 mol of dihydroxymethyl was slowly added to the second mixture.

[0157] Bisphenol A, control the reaction temperature to 70 ° C, react under reflux for 4.5 hours to obtain an intermediate, use 5-triethanolamine to neutralize the intermediate, reduce the pressure and vacuum for 30 minutes to remove toluene, discharge the material, and obtain a cross-linking agent.

[0158] The structural formula of dihydroxymethyl bisphenol A is as follows:

[0159]

[0160] The structural formula of the crosslinking agent is as follows:

[0161]

[0162] A negative chemically amplified photoresist composition comprises 11.02g of poly(p-hydroxystyrene) resin, 0.756g of trifluoromethanesulfonate sulfonium salt, 0.756g of the above cross-linking agent, 5.04g of 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g of 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 51.35g of 1,2-propylene glycol methyl ether acetate. The above substances are weighed and mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0163] Example 2

[0164] The embodiment of the present application provides a cross-linking agent and a preparation method thereof, and a photoresist, which comprises the following steps:

[0165] 1.0 mol of octylphenol, 2.0 mol of dodecanol and 100 mL of xylene were added to a 500 mL round-bottom flask equipped with a stirring device, a thermometer and a reflux condenser, the temperature was raised and stirred to completely dissolve the octylphenol and dodecanol in the xylene to obtain a first mixture, 0.5 g of dodecylbenzenesulfonic acid was added to the first mixture to obtain a second mixture, 1.0 mol of trimethylolbisphenol A was slowly added to the second mixture, the reaction temperature was controlled to 70° C., the reaction was carried out under reflux for 4.5 hours to obtain an intermediate, the intermediate was neutralized with triethanolamine, the xylene was removed by vacuuming for 30 minutes, and the material was discharged to obtain a cross-linking agent.

[0166] The structural formula of trimethylolbisphenol A is as follows:

[0167]

[0168] The structural formula of the crosslinking agent is as follows:

[0169]

[0170] A negative chemically amplified photoresist composition comprises 11.02g of poly(p-hydroxystyrene) resin, 0.756g of trifluoromethanesulfonate sulfonium salt, 0.756g of the above cross-linking agent, 5.04g of 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g of 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 51.35g of 1,2-propylene glycol methyl ether acetate. The above substances are weighed and mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0171] Example 3

[0172] The embodiment of the present application provides a cross-linking agent and a preparation method thereof, and a photoresist, which comprises the following steps:

[0173] 1.0 mol of dodecylphenol, 1.0 mol of ethanol and 100 mL of toluene were added to a 500 mL round-bottom flask equipped with a stirring device, a thermometer and a reflux condenser, the temperature was raised and stirred to completely dissolve the dodecylphenol and ethanol in the toluene to obtain a first mixture, 0.5 g of dodecylbenzenesulfonic acid was added to the first mixture to obtain a second mixture, 1.0 mol of dihydroxymethylbisphenol A was slowly added to the second mixture, the reaction temperature was controlled to 70° C., the reaction was carried out under reflux for 4.5 hours to obtain an intermediate, the intermediate was neutralized with triethanolamine, the toluene was removed by vacuuming for 30 minutes, and the material was discharged to obtain a cross-linking agent.

[0174] The structural formula of dihydroxymethyl bisphenol A is as follows:

[0175]

[0176] The structural formula of the crosslinking agent is as follows:

[0177]

[0178] A negative chemically amplified photoresist composition comprises 11.02g of poly(p-hydroxystyrene) resin, 0.756g of trifluoromethanesulfonate sulfonium salt, 0.756g of the above cross-linking agent, 5.04g of 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g of 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 51.35g of 1,2-propylene glycol methyl ether acetate. The above substances are weighed and mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0179] Example 4

[0180] The embodiment of the present application provides a cross-linking agent and a preparation method thereof, and a photoresist, which comprises the following steps:

[0181] 1.0 mol of dodecylphenol, 1.0 mol of eicosanol and 100 mL of toluene were added to a 500 mL round-bottom flask equipped with a stirring device, a thermometer and a reflux condenser, the temperature was raised and stirred to completely dissolve the dodecylphenol and eicosanol in the toluene to obtain a first mixture, 0.5 g of dodecylbenzenesulfonic acid was added to the first mixture to obtain a second mixture, 1.0 mol of dihydroxymethylbisphenol A was slowly added to the second mixture, the reaction temperature was controlled to 70° C., the reaction was carried out under reflux for 4.5 hours to obtain an intermediate, the intermediate was neutralized with triethanolamine, the toluene was removed by vacuuming for 30 minutes, and the material was discharged to obtain a cross-linking agent.

[0182] The structural formula of dihydroxymethyl bisphenol A is as follows:

[0183]

[0184] The structural formula of the crosslinking agent is as follows:

[0185]

[0186] A negative chemically amplified photoresist composition comprises 11.02g of poly(p-hydroxystyrene) resin, 0.756g of trifluoromethanesulfonate sulfonium salt, 0.756g of the above cross-linking agent, 5.04g of 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g of 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 51.35g of 1,2-propylene glycol methyl ether acetate. The above substances are weighed and mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0187] Example 5

[0188] The embodiment of the present application provides a cross-linking agent and a preparation method thereof, and a photoresist, which comprises the following steps:

[0189] 2.0 mol of octylphenol, 2.0 mol of dodecanol and 100 mL of xylene were added to a 500 mL round-bottom flask equipped with a stirring device, a thermometer and a reflux condenser, the temperature was raised and stirred to completely dissolve tetradecylphenol and n-octanol in the xylene to obtain a first mixture, 0.5 g of dodecylbenzenesulfonic acid was added to the first mixture to obtain a second mixture, 1.0 mol of tetrahydroxymethylbisphenol A was slowly added to the second mixture, the reaction temperature was controlled to 70° C., the reaction was carried out under reflux for 4.5 hours to obtain an intermediate, the intermediate was neutralized with triethanolamine, the xylene was removed by vacuuming for 30 minutes, and the material was discharged to obtain a cross-linking agent.

[0190] The structural formula of tetrahydroxymethyl bisphenol A is as follows:

[0191]

[0192] The structural formula of the crosslinking agent is as follows:

[0193]

[0194] A negative chemically amplified photoresist composition comprises 11.02g of poly(p-hydroxystyrene) resin, 0.756g of trifluoromethanesulfonate sulfonium salt, 0.756g of the above cross-linking agent, 5.04g of 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g of 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 51.35g of 1,2-propylene glycol methyl ether acetate. The above substances are weighed and mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0195] Example 6

[0196] The embodiment of the present application provides a cross-linking agent and a preparation method thereof, and a photoresist, which comprises the following steps:

[0197] 1.0 mol of dodecylphenol, 2.0 mol of n-octanol and 100 mL of toluene were added to a 500 mL round-bottom flask equipped with a stirring device, a thermometer and a reflux condenser, the temperature was raised and stirred to completely dissolve the dodecylphenol and n-octanol in the toluene to obtain a first mixture, 0.5 g of dodecylbenzenesulfonic acid was added to the first mixture to obtain a second mixture, 1.0 mol of 1,5-dihydroxymethylbisphenol A was slowly added to the second mixture, the reaction temperature was controlled to 70° C., the reaction was carried out under reflux for 4.5 hours to obtain an intermediate, the intermediate was neutralized with triethanolamine, the toluene was removed by vacuuming for 30 minutes, and the material was discharged to obtain a cross-linking agent.

[0198] The structural formula of 1,5-dihydroxymethylbisphenol A is as follows:

[0199]

[0200] The structural formula of the crosslinking agent is as follows:

[0201]

[0202] A negative chemically amplified photoresist composition comprises 11.02g of poly(p-hydroxystyrene) resin, 0.756g of trifluoromethanesulfonate sulfonium salt, 0.756g of the above cross-linking agent, 5.04g of 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g of 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 51.35g of 1,2-propylene glycol methyl ether acetate. The above substances are weighed and mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0203] Example 7

[0204] The embodiment of the present application provides a cross-linking agent and a preparation method thereof, and a photoresist, which comprises the following steps:

[0205] 1.0 mol of dodecylphenol, 1.0 mol of n-octanol and 100 mL of toluene were added to a 500 mL round-bottom flask equipped with a stirring device, a thermometer and a reflux condenser, the temperature was raised and stirred to completely dissolve the dodecylphenol and n-octanol in the toluene to obtain a first mixture, 0.5 g of dodecylbenzenesulfonic acid was added to the first mixture to obtain a second mixture, 1.0 mol of 1,5-dihydroxymethyl-p-tert-butylphenol was slowly added to the second mixture, the reaction temperature was controlled to 70° C., the reaction was carried out under reflux for 4.5 hours to obtain an intermediate, the intermediate was neutralized with triethanolamine, the toluene was removed by vacuuming for 30 minutes under reduced pressure, and the material was discharged to obtain a cross-linking agent.

[0206] The structural formula of 1,5-dihydroxymethyl-4-tert-butylphenol is as follows:

[0207]

[0208] The structural formula of the crosslinking agent is as follows:

[0209]

[0210] A negative chemically amplified photoresist composition comprises 11.02g of poly(p-hydroxystyrene) resin, 0.756g of trifluoromethanesulfonate sulfonium salt, 0.756g of the above cross-linking agent, 5.04g of 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g of 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 51.35g of 1,2-propylene glycol methyl ether acetate. The above substances are weighed and mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0211] Comparative Example 1

[0212] The comparative example of the present application provides a cross-linking agent and a photoresist, and the structural formula thereof is as follows:

[0213]

[0214] A negative chemically amplified photoresist composition comprises 11.02g of poly(p-hydroxystyrene) resin, 0.756g of trifluoromethanesulfonate sulfonium salt, 0.756g of the above cross-linking agent, 5.04g of 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g of 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 51.35g of 1,2-propylene glycol methyl ether acetate. The above substances are weighed and mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0215] Comparative Example 2

[0216] The embodiment of the present application provides a cross-linking agent and a preparation method thereof, and a photoresist, which comprises the following steps:

[0217] 1.0 mol of dodecylphenol and 100 mL of toluene were added to a 500 mL round-bottom flask equipped with a stirring device, a thermometer and a reflux condenser, the temperature was raised and stirred to completely dissolve the dodecylphenol in the toluene to obtain a first mixture, 0.5 g of dodecylbenzenesulfonic acid was added to the first mixture to obtain a second mixture, 1.0 mol of monohydroxymethylbisphenol A was slowly added to the second mixture, the reaction temperature was controlled to 70° C., the reaction was carried out under reflux for 4.5 hours to obtain an intermediate, the intermediate was neutralized with triethanolamine, the toluene was removed by vacuuming for 30 minutes, and the material was discharged to obtain a cross-linking agent.

[0218] The structural formula of monohydroxymethyl bisphenol A is as follows:

[0219]

[0220] The structural formula of the crosslinking agent is as follows:

[0221]

[0222] A negative chemically amplified photoresist composition comprises 11.02g of poly(p-hydroxystyrene) resin, 0.756g of trifluoromethanesulfonate sulfonium salt, 0.756g of the above cross-linking agent, 5.04g of 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g of 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 51.35g of 1,2-propylene glycol methyl ether acetate. The above substances are weighed and mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0223] Test Example 1

[0224] The photoresists of Examples 1 to 7 and Comparative Examples 1 to 2 were spin-coated on an 8-inch single crystal silicon wafer. After coating, the substrate coated with the photoresist was pre-baked on a hot plate at 100°C / 60s, and the rotation speed was adjusted so that the film thickness after drying was 0.6μm. The substrate was then exposed using a DUV exposure machine. The exposed substrate was post-baked on a hot plate at 115°C / 60s, and finally the substrate was spray-developed with 2.38wt% tetramethylammonium hydroxide for 60s. After the operation was completed, the patterns formed after development were compared using CD-SEM (Hitachi S9220) and X-SEM (S4800), as shown in FIG. Figures 3 to 10 shown.

[0225] Depend on Figures 3-4 It can be seen that the crosslinking agent of Examples 1 to 2 of the present application can make the crosslinking reaction of the base resin of the photoresist more uniform, and significantly improve the morphological defects caused by excessive local molecular weight (such as Figure 1 and Figure 2 As shown), the edges of the obtained graphic lines are more vertical and the window is 0.6μm.

[0226] Depend on Figures 5-6 It can be seen that the R13 groups of the cross-linking agents of Examples 3 to 4 of the present application are C2 alkyl and C20 alkyl, and the edges of the obtained graphic lines are relatively vertical, and the window is 0.4 μm.

[0227] Depend on Figure 7 It can be seen that the cross-linking agent of Example 5 of the present application has 5 groups selected from at least one of the first group and the second group, and the edge portion of the obtained graphic line is not very vertical, and the window is 0.3 μm.

[0228] Depend on Figure 8 It can be seen that all the first groups and the second groups in the cross-linking agent of Example 6 of the present application are connected to the same benzene ring structure, and the edge of the obtained graphic line is not very vertical, and the window is 0.3 μm.

[0229] Depend on Fig. 9It can be seen that there is only one benzene ring structure in the cross-linking agent of Example 7 of the present application, and all the first groups and second groups are connected to this benzene ring structure. The edge of the obtained graphic line is not very vertical, and the window is 0.3μm.

[0230] Depend on Fig.10 It can be seen that the cross-linking agent in Comparative Example 1 of the present application is an existing cross-linking agent, and the edges of the obtained graphic lines are mostly not vertical, and the window is only 0.2 μm.

[0231] The cross-linking agent in Comparative Example 2 of the present application cannot cause the base resin of the photoresist to undergo a cross-linking reaction, and thus cannot form a pattern.

[0232] Test Example 2

[0233] The photoresist of Example 1 and Example 3 was re-prepared, and the formula was: 11.02g poly(p-hydroxystyrene) resin, 0.756g trifluoromethanesulfonate sulfonium salt, 0.756g cross-linking agent, 5.04g 1wt% triethanolamine 1,2-propylene glycol methyl ether acetate solution, 1.07g 1wt% surfactant BYK307 1,2-propylene glycol methyl ether acetate solution, and 12.85g 1,2-propylene glycol methyl ether acetate. The above substances were weighed, mixed, stirred thoroughly to completely dissolve, and filtered through a 0.1μm polytetrafluoroethylene microporous filter membrane to obtain a negative chemically amplified photoresist.

[0234] The photoresists of Example 1 and Example 3 were spin-coated on an 8-inch single crystal silicon wafer. After coating, the substrate coated with the photoresist was pre-baked on a hot plate at 120°C / 180s. The rotation speed was adjusted so that the film thickness after drying was 20.0μm. The substrate was then exposed using a DUV exposure machine. The exposed substrate was post-baked on a hot plate at 110°C / 60s. Finally, the substrate was spray-developed with 2.38wt% tetramethylammonium hydroxide for 60s. After the operation was completed, the patterns formed after development were compared using CD-SEM (Hitachi S9220) and X-SEM (S4800). Fig.11 and 12 shown.

[0235] By comparing Example 1 and Example 3, it can be seen that there is no cracking between the photoresist layer and the substrate in Example 1, but there is cracking between the photoresist layer and the substrate in Example 3. That is, the cross-linking agent in Example 1 of the present application can alleviate the stress problem between the substrate and the photoresist caused by hard film by adjusting the structure of the cross-linking agent active group and the number of active sites, thereby reducing the risk of deformation and cracking of the photoresist layer.

[0236] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A photoresist, characterized in that: The photoresist comprises: a solute and a first solvent, wherein the solute comprises 70wt% to 95wt% of an alkali-soluble resin, 1wt% to 30wt% of a photoacid generator, 5wt% to 20wt% of a cross-linking agent, and 0.1wt% to 15wt% of an acid quencher, and the mass of the first solvent is 1 to 10 times the mass of the alkali-soluble resin; The structural formula of the cross-linking agent is as follows: Wherein, the R1, the R2, the R3, the R4 and the R5 are each independently selected from H, OH, or -R 12 -OR 13 ; The R6 is selected from C 1~10 alkyl; The R7, R8 and R9 are each independently selected from H, C 1~6 Saturated or unsaturated alkyl, C 1~6 Saturated or unsaturated cycloalkyl, 、-OR 15 or ; The R 10 Selected from C 1~5 alkyl; The R 11 Selected from C 1~20 alkyl; The R 12 Selected from C 1~5 alkyl; The R 13 Selected from C 8~14 alkyl; The R 14 Selected from C 1~20 alkyl; The R 15 Selected from C 8~14 alkyl; The R 16 , the R 17 , the R 18 , the R 19 and the R 20 Each independently selected from H, OH, or -R 12 -OR 13 ; R1, R2, R3, R4, R5, R 16 , the R 17 , the R 18 , the R 19 and the R 20 At least two of any of , part of which are selected from the first group and part of which are selected from the second group; The structural formula of the first group is ; The structural formula of the second group is -R 12 -OR 13 , and the R 13 Not for H.

2. The photoresist according to claim 1, characterized in that R1, R2, R3, R4, R5, R 16 , the R 17 , the R 18 , the R 19 and the R 20 Any 1 to 5 of them are selected from OH.

3. The photoresist according to claim 1, characterized in that The R 10 Selected from CH2.

4. The photoresist according to claim 1, characterized in that The R9 is selected from .

5. The photoresist according to claim 1, characterized in that The alkali-soluble resin includes any one or more of poly(p-hydroxystyrene) resin, polystyrene resin, poly(p-hydroxystyrene) resin and linear phenolic resin.

6. The photoresist according to claim 1, characterized in that The photoacid generator includes any one or more of iodonium salts, sulfonium salts and heterocyclic acid generators.

7. The photoresist according to claim 1, characterized in that The acid quencher includes a basic organic substance.

8. The photoresist according to claim 7, characterized in that The alkaline organic matter includes tertiary ammonium and / or quaternary ammonium compounds.

9. The photoresist according to claim 1, characterized in that The first solvent includes any one or more of 1,2-propylene glycol methyl ether acetate, ethyl lactate and ethyl acetate.

10. The photoresist according to claim 1, characterized in that The preparation method of the cross-linking agent comprises: subjecting a hydroxyalkylphenol compound and a reactant to an acidic catalytic reaction to obtain an intermediate, and then neutralizing the intermediate; The structural formula of the hydroxyalkylphenol compound is as follows: Among them, the R 21 , the R 22 , the R 23 , the R 24 and the R 25 Each independently selected from H, OH or -R 12 -OH; The R 12 Selected from C 1~10 alkyl; The R 26 Selected from C 1~10 alkyl; The R 27 , the R 28 and the R 29 Each independently selected from H, C 1~6 Saturated or unsaturated alkyl, C 1~6 Saturated or unsaturated cycloalkyl or ; The R 30 , the R 31 , the R 32 , the R 33 and the R 34 Each independently selected from H, OH or -R 35 -OH; The R 35 Selected from C 1~10 alkyl; The R 21 , the R 22 , the R 23 , the R 24 , the R 25 , the R 30 , the R 31 , the R 32 , the R 33 and the R 34 Any at least two of the group consisting of at least one of the third group and the fourth group; The structural formula of the third group is -R 12 -OH; The structural formula of the fourth group is -R 35 -OH; The reactant includes at least one of an alkylphenol compound and an alcohol compound; The structural formula of the alkylphenol compound is as follows: Among them, the R 36 , the R 37 Each independently selected from H or -R 38 ; The R 38 Selected from C 1-20 Saturated or unsaturated alkyl; The R 36 , the R 37 Any at least one selected from -R 38 ; The structural formula of the alcohol compound is as follows: The n is 0~19.

11. The photoresist according to claim 10, characterized in that The acidic catalytic reaction temperature is 50° C. to 150° C., and the reaction time is 0.4 h to 12 h.

12. The photoresist according to claim 11, characterized in that The molar ratio of the hydroxyalkylphenol compound to the reactant is 1:2 to 1:4.

Citation Information

Patent Citations

  • Phenolic epoxy compounds

    CN105121495A

  • Resist underlayer film forming composition containing substituted crosslinkable compound

    CN105324720A

  • Polyimide varnish

    JP2008308572A