Preparation method and application of Pt single-atom catalyst for thermal catalytic CO2 reduction

By preparing a highly stable Pt/Zn2Al1-MMO catalyst, combined with the platinum single atom active site, the problem of poor high temperature stability in the anti-water vapor transformation reaction is solved, and efficient carbon dioxide conversion and carbon monoxide selectivity is achieved, satisfying the satisfaction of The requirements for industrial application are met.

CN115957753BActive Publication Date: 2024-11-22BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310110035.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-14
Publication Date
2024-11-22
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

The existing non-precious metal catalysts have problems of poor high temperature stability and low activity in the reverse water vapor transformation reaction, which cannot meet the requirements of industrial applications.

Method used

Using the preparation method of Pt/Zn2Al1-MMO catalyst, the mixed solution of zinc salt and aluminum salt is dispersed by ultrasonic dispersion, sodium hydroxide and sodium carbonate solution are added to form the precursor of Zn2Al1-LDHs catalyst, and the Zn2Al1-MMO catalyst is obtained by calcination. Binding with the platinum single atom active site, a high stability Pt/Zn2Al1-MMO mixed oxide catalyst is formed.

Benefits of technology

Improve carbon monoxide selectivity and carbon dioxide conversion rate. At 600℃, the carbon dioxide conversion rate is higher than 50%, the carbon monoxide selectivity is as high as 96% to 99%, and the conversion rate can reach 50% for 12 hours of reaction at high aerial speed, showing excellent performance catalytic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115957753B_ABST
    Figure CN115957753B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method and application of a Pt single-atom catalyst for thermal catalytic CO2 reduction, and realizes high selectivity and high stability of reverse water vapor shift reaction. The present invention uses zinc nitrate hexahydrate and aluminum nitrate nonahydrate as raw materials, prepares Zn2Al1-LDHs as a precursor of the catalyst by coprecipitation, further calcines at 500°C in air to obtain Zn2Al1-MMO composite oxide, adopts an equal volume impregnation method to load different loads of precious metal Pt, and finally calcines at high temperature to form a Pt single-atom catalyst loaded by Zn2Al1-MMO composite oxide. The catalyst obtained by the present invention has a simple process, shows good high temperature stability and activity for reverse water vapor shift reaction, effectively solves the problems of low product selectivity and poor stability during the reaction, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-temperature stable supported noble metal catalyst and a preparation method thereof, in particular to the preparation of a single-atom Pt-based catalyst and its application in a reverse water vapor shift reaction. Background Art

[0002] With the growth of the global population and the acceleration of industrialization, global carbon dioxide emissions have risen sharply since the last century. Environmental problems such as seawater acidification and climate warming caused by large-scale carbon dioxide emissions are becoming increasingly serious and have become one of the social problems that need to be solved urgently. Research on the resource utilization of CO2 undoubtedly provides great theoretical value and practical needs for solving energy problems and reducing CO2 emissions. Reverse water gas shift reaction (RWGS) is one of the most effective ways to achieve CO2 resource utilization. The route of producing CO through this reaction may be the best solution to replace traditional coal chemical production of synthesis gas, and is expected to become the basis for the future development of green coal chemical technology.

[0003] Non-precious metal catalysts have poor high-temperature stability and easy sintering and deactivation in the RWGS reaction. Although the addition of alkaline metals, transition metals, etc. as electronic and structural additives can inhibit catalyst deactivation to a certain extent, they cannot meet the requirements of industrial application due to their poor high-temperature stability and short lifespan. In 2012, researchers used 1% loaded Pt / TiO2 and Pt / Al2O3 to carry out reverse water gas shift reaction, proving that the catalyst that Pt can catalyze water gas shift can also catalyze its reverse reaction, with the advantage of high selectivity but low conversion rate. In view of the above shortcomings, a Pt / Zn2Al1-MMO catalyst with high stability and product selectivity and its preparation method are urgently needed in the industry. Summary of the invention

[0004] In view of the problems of poor stability and low activity in the prior art, the present invention provides a method for preparing a highly stable Pt / Zn2Al1-MMO catalyst and applies it to the reverse water gas shift reaction. The present invention is achieved by the following technical means:

[0005] The present invention discloses a method for preparing a Pt / Zn2Al1-MMO catalyst, and the specific steps are as follows:

[0006] (1) preparing a mixed solution of a soluble zinc salt and a soluble aluminum salt with deionized water, and then dispersing the mixed solution by ultrasonication to obtain a first solution;

[0007] (2) preparing a mixed solution of sodium hydroxide and sodium carbonate with deionized water, and then dispersing by ultrasonication to obtain a second solution;

[0008] (3) adding the first solution and the second solution into a three-necked flask, stirring, washing, drying and grinding at a certain speed at 85° C. to obtain a Zn2Al1-LDHs catalyst precursor, i.e., the third product;

[0009] (4) calcining the third product to obtain a Zn2Al1-MMO catalyst;

[0010] (5) Weigh the required amount of active component Pt precursor solution into a beaker, add deionized water to prepare a third solution, weigh the catalyst support Zn2Al1-MMO obtained in step (4), add the prepared third solution thereto, stir for 4 hours, dry, and grind to obtain a fourth product;

[0011] (6) The fourth product is calcined at high temperature to obtain a Pt / Zn2Al1-MMO mixed oxide catalyst.

[0012] Furthermore, the Zn salt in step (1) is selected from any one of zinc nitrate and zinc chloride.

[0013] Furthermore, the Al salt in step (1) is selected from any one of aluminum nitrate and aluminum chloride.

[0014] Furthermore, the ultrasonic dispersion time in step (1) is 30 minutes.

[0015] Furthermore, the molar amount of sodium carbonate in step (2) is twice the total molar amount of aluminum ions in the first solution.

[0016] Furthermore, the molar amount of the sodium hydroxide in step (2) is 1.6 times the total molar amount of cations in the first solution.

[0017] Furthermore, the ultrasonic dispersion time in step (2) is 30 minutes.

[0018] Furthermore, the stirring time in step (3) is 24 hours.

[0019] Furthermore, the calcination condition in step (4) is calcination at 500° C. for 4 hours in an air atmosphere.

[0020] Furthermore, the Pt precursor solution used in step (5) is H2PtCl 6* Any one of 6H2O, PtCl4, Pt(NO3)2, concentration 5-100mgmL -1 .

[0021] Furthermore, the calcination conditions in step (6) are calcination at 400-1200° C. for 1-4 h in air atmosphere.

[0022] The invention also discloses a Pt / Zn2Al1-MMO catalyst prepared according to any one of the above preparation methods.

[0023] The invention also discloses an application of the Pt / Zn2Al1-MMO catalyst in a reverse water-gas shift reaction process.

[0024] Further, the conditions of the reverse water gas shift reaction are:

[0025] Under normal pressure conditions, the reverse water-gas shift reaction evaluation device is a fixed-bed reactor;

[0026] The raw gas includes: 20% carbon dioxide, 60% hydrogen, and 20% nitrogen by volume, and the catalyst loading is 0.01-1000g; the reaction temperature is 100-1000℃, and the space velocity is 3000-2000000mL·g -1 ·h -1 .

[0027] The beneficial effects of the present invention are:

[0028] The Pt / Zn2Al1-MMO catalyst prepared by the present invention improves the carbon monoxide selectivity and the carbon dioxide conversion rate through the platinum single atom active site. Therefore, it shows good catalytic performance in the reverse water vapor shift reaction. At 600°C, the carbon dioxide conversion rate is higher than 50%, the carbon monoxide selectivity is as high as 96% to 99%, and the conversion rate can reach 50% after 12 hours of reaction at high space velocity. Compared with the prior art, the reverse water vapor shift reaction catalyst provided by the present invention is excellent, has the advantages of simple synthesis method and low production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a high-resolution electron microscope photograph of the 3% Pt / Zn2Al1-MMO single-atom catalyst obtained in Example 3 of the present invention.

[0030] Figure 2 This is the extended edge X-ray absorption fine structure of the 3% Pt / Zn2Al1-MMO catalyst obtained in Example 3 of the present invention.

[0031] Figure 3 It is a comparative performance diagram of the catalysts obtained in Examples 1, 2 and 3 of the present invention.

[0032] Figure 4 This is a performance diagram of the 3% Pt / Zn2Al1-MMO single atom catalyst obtained in Example 3 of the present invention.

[0033] Figure 5 This is a stability performance test chart of the 3% Pt / Zn2Al1-MMO single atom catalyst obtained in Example 3 of the present invention under high space velocity conditions. DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of a method for preparing a Pt / Zn2Al1-MMO catalyst of the present invention is further explained below in conjunction with the accompanying drawings and through specific implementation methods.

[0035] Example 1

[0036] A preparation method of 0.5% Pt / Zn2Al1-MMO catalyst, the specific steps are as follows:

[0037] First, add 0.3 mol zinc nitrate and 0.1 mol aluminum nitrate mixed solution to 60 mL deionized water and stir for 30 minutes, and prepare 1.6 times the total molar amount of cations of sodium hydroxide and 2 times the molar amount of trivalent cations of sodium carbonate mixed solution with 60 mL deionized water and stir for 30 minutes; add 60 mL deionized water to a three-necked flask, transfer the two mixed solutions to a constant pressure low liquid funnel, drop them into the three-necked flask, stir at 85 ° C for 24 hours, and obtain a Zn2Al1-LDHs catalyst precursor; after washing, drying and grinding, the obtained product is placed in a muffle furnace at 5 ° C min -1 Heat to 500℃ and calcine for 4h to obtain Zn2Al1-MMO product. Take 300mg Zn2Al1-MMO powder in a 5mL single-necked flask and add 5mgmL -1 H2PtCl 6* 0.796 mL of 6H2O solution was taken and dropped into a single-necked flask, and then 2.204 mL of deionized water was added and stirred for 4 h. The obtained product was dried and ground and then heated in a muffle furnace at 5 °C min -1 Heat to 900℃, keep warm for 4h and then increase the temperature by 10℃min -1 Cool down to room temperature. Reverse water vapor shift reaction Weigh 0.1 g of catalyst to react.

[0038] Example 2

[0039] A method for preparing a 1% Pt / Zn2Al1-MMO catalyst, the specific steps are as follows:

[0040] First, add 0.3 mol zinc nitrate and 0.1 mol aluminum nitrate mixed solution to 60 mL deionized water and stir for 30 minutes, and prepare 1.6 times the total molar amount of cations of sodium hydroxide and 2 times the molar amount of trivalent cations of sodium carbonate mixed solution with 60 mL deionized water and stir for 30 minutes; add 60 mL deionized water to a three-necked flask, transfer the two mixed solutions to a constant pressure low liquid funnel, drop them into the three-necked flask, stir at 85 ° C for 24 hours, and obtain a Zn2Al1-LDHs catalyst precursor; after washing, drying and grinding, the obtained product is placed in a muffle furnace at 5 ° C min -1Heat to 500℃ and calcine for 4h to obtain Zn2Al1-MMO product. Take 300mg Zn2Al1-MMO powder in a 5mL single-necked flask and add 5mgmL -1 H2PtCl 6* 1.593 mL of 6H2O solution was taken and dropped into a single-necked flask, and then 1.407 mL of deionized water was added and stirred for 4 h. The obtained product was dried and ground and then heated in a muffle furnace at 5 °C min -1 Heat to 900℃, keep warm for 4h and then increase the temperature by 10℃min -1 Cool down to room temperature. Reverse water vapor shift reaction Weigh 0.1 g of catalyst to react.

[0041] Example 3

[0042] A preparation method of a 3% Pt / Zn2Al1-MMO catalyst, the specific steps are as follows:

[0043] First, add 0.3 mol zinc nitrate and 0.1 mol aluminum nitrate mixed solution to 60 mL deionized water and stir for 30 minutes, and prepare 1.6 times the total molar amount of cations of sodium hydroxide and 2 times the molar amount of trivalent cations of sodium carbonate mixed solution with 60 mL deionized water and stir for 30 minutes; add 60 mL deionized water to a three-necked flask, transfer the two mixed solutions to a constant pressure low liquid funnel, drop them into the three-necked flask, stir at 85 ° C for 24 hours, and obtain a Zn2Al1-LDHs catalyst precursor; after washing, drying and grinding, the obtained product is placed in a muffle furnace at 5 ° C min -1 Heat to 500℃, calcine for 4h to obtain Zn2Al1-MMO product. Take 300mgZn2Al1-MMO powder in a 5mL single-necked flask and add 10mgmL -1 H2PtCl 6* 2.389 mL of 6H2O solution was taken and dropped into a single-necked flask, and then 0.611 mL of deionized water was added. The obtained product was dried and ground and then heated in a muffle furnace at 5 °C min -1 Heat to 900℃, keep warm for 4h and then increase the temperature by 10℃min -1 Cool down to room temperature. Reverse water vapor shift reaction Weigh 0.1 g of catalyst to react.

[0044] The HRTEM image of the 3% Pt / Zn2Al1-MMO single atom catalyst obtained in this example is attached. Figure 1 .from Figure 1 It can be seen that ZnO and Al2O3 are uniformly dispersed.

[0045] Figure 2The X-ray absorption near edge structure spectrum (XANES) and the corresponding Fourier transform spectrum (FT-EXAFS) of the Pt element of the 3% Pt / Zn2Al1-MMO single atom catalyst obtained in this example are as follows: Figure 2 As shown, single-atom Pt was formed.

[0046] Figure 3 3 is a comparative performance diagram of the catalysts obtained in Examples 1, 2 and 3 of the present invention. As shown in the figure, the 3% Pt / Zn2Al1-MMO catalyst has relatively good catalytic performance.

[0047] Figure 4 This is the conversion rate and selectivity of 3% Pt / Zn2Al1-MMO single atom catalyst, and the CO selectivity is close to 100%.

[0048] Figure 5 It shows that 3% Pt / Zn2Al1-MMO single atom catalyst has a high thermal conductivity at a space velocity of 120000 mL·g -1 ·h -1 , 240000mL·g -1 ·h -1 , 480000mL·g -1 ·h -1 It still has good catalytic activity.

[0049] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. Application of a Pt / Zn2Al1-MMO mixed oxide catalyst in a reverse water gas shift reaction process, characterized in that: The reverse water gas shift reaction conditions include: Under normal pressure conditions, the reverse water-steam shift reaction evaluation device is a fixed-bed reactor; The raw material gas includes: 20% by volume of carbon dioxide, 60% by volume of hydrogen, and 20% by volume of nitrogen; The catalyst loading is 0.01-1000g; The reaction temperature is 600-1000°C; Space velocity is 120000-2000000mL·g -1 ·h -1 ;in: The Pt / Zn2Al1-MMO mixed oxide catalyst is prepared by the following method: (1) preparing a mixed solution of a soluble zinc salt and a soluble aluminum salt with deionized water, and then dispersing the mixed solution by ultrasonication to obtain a first solution; (2) preparing a mixed solution of sodium hydroxide and sodium carbonate with deionized water, and then dispersing by ultrasonication to obtain a second solution; (3) The first solution and the second solution are transferred to a constant pressure low liquid funnel respectively, and are simultaneously dripped into a three-necked flask, stirred at 85° C., washed, dried, and ground to obtain a third product; (4) The third product is calcined to obtain a Zn2Al1-MMO catalyst; (5) Weigh the active component Pt precursor solution into a beaker, add deionized water to prepare a third solution, weigh the Zn2Al1-MMO catalyst, drop the third solution into it, stir for 4 hours, and dry to obtain a fourth product; (6) The fourth product was calcined at 900°C for 4 h in an air atmosphere to obtain a Pt / Zn2Al1-MMO mixed oxide catalyst.

2. The use according to claim 1, characterized in that: The Zn salt in step (1) is selected from any one of zinc nitrate and zinc chloride; The Al salt is selected from any one of aluminum nitrate and aluminum chloride; The ultrasonic dispersion time is 30 min.

3. The use according to claim 1, characterized in that: The molar amount of sodium carbonate in step (2) is twice the total molar amount of aluminum ions in the first solution; The molar amount of the sodium hydroxide is 1.6 times the total molar amount of cations in the first solution; The ultrasonic dispersion time is 30 min.

4. The use according to claim 1, characterized in that: The stirring time in step (3) is 24 hours.

5. The use according to claim 1, characterized in that: The calcination conditions of step (4) are: calcination at 500° C. for 4 h in air atmosphere.

6. The use according to claim 1, characterized in that: The Pt precursor used in step (5) is any one of H2PtCl6·6H2O, PtCl4, Pt(NO3)2, with a concentration of 5-10 mg·mL -1 .