A method for controlling the carbon content of cemented carbide and a method for preparing cemented carbide

By determining the carbon content adjustment under the limit range of carbon windows and humidity conditions in cemented carbides, combined with plasma spraying and sintering technology, the decarbonization and carburization problems caused by unbalanced carbon content in cemented carbides are solved, and the quality of the product is improved Stability and pass rate.

CN115971489BActive Publication Date: 2024-11-22CHONGYI ZHANGYUAN TUNGSTEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310168356.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-11-22
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

The uneven carbon content in cemented carbide leads to decarbonization and carburization of products, affecting the density, strength and hardness of products. In addition, the products have different degrees of decarbonization and carburization problems in different seasons and climate conditions, making it difficult to be effective. control.

Method used

By determining the magnetic saturation strength range of the carbon window limit range of the two-phase area of ​​cemented carbide, and controlling the carbon content according to the humidity RH of the production environment, plasma spraying and fully coated boat dishes are used for sintering. The specific steps include different Adjust the carbon content and sintering time under humidity conditions to reduce the risk of decarbonization and carburization.

Benefits of technology

It effectively reduces the probability of the product appearing in three-phase zones, improves the stability of the carbon atmosphere, improves the quality stability and pass rate of the product, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of powder metallurgy, and specifically relates to a method for controlling the carbon content of cemented carbide and a method for preparing cemented carbide. According to the magnetic saturation intensity range COM of the carbon window limit range of the two-phase region of qualified cemented carbide products, L ~COM H As well as the humidity RH of the production environment, the carbon content of the cemented carbide is controlled, which reduces the probability of the three-phase zone appearing in the product. At the same time, the use of plasma sprayed fully coated boats for sintering will not cause carbon escape, which reduces the interference of the carbon atmosphere during the sintering process, improves the stability of the carbon atmosphere, and further promotes the quality stability of the product in long-term production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy, and specifically relates to a method for controlling the carbon content of cemented carbide and a method for preparing cemented carbide. Background Art

[0002] Because of its good hardness and strength, cemented carbide is widely used in mining, mechanical processing, mold materials and other fields. However, the carbon content in cemented carbide is regarded as the lifeline of cemented carbide. Too high or too low will lead to unqualified products. When the carbon content is too high, carburization will occur in the product. Carburization means the appearance of graphite phase in the product, making the product present three phases, and the density, strength, hardness and other properties of the product will be greatly reduced. When the carbon content is too low, the product will cause the decarburization phase composed of C, W and Co. The appearance of the decarburization phase will lead to reduced strength, high brittleness, and the formation of fracture sources, which will reduce the life of the product. Researchers have done a lot of research on the control of the carbon content of cemented carbide. In actual production, cemented carbide manufacturers will form different standard production processes for different products. Even so, due to different seasons and different climatic conditions, the product will have different degrees of decarburization and carburization problems. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to propose a method for controlling the carbon content of cemented carbide and a method for preparing cemented carbide, which can reduce the risk of large-scale decarburization and carburization problems in products and improve the product qualification rate.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A method for controlling the carbon content of cemented carbide comprises the following steps:

[0006] S1. Determine the magnetic saturation intensity range COM of the carbon window limit range of the cemented carbide two-phase region L ~COM H ;

[0007] S2. According to the different production environment humidity RH, based on the magnetic saturation intensity range COM of step S1 L ~COM H Control the carbon content of cemented carbide, specifically:

[0008] When the humidity RH>85%, the magnetic saturation intensity of cemented carbide is (COM L +1.15×COM H ) / 2 when the corresponding carbon content is used for carbon matching;

[0009] When 55<humidity RH≤85%, the magnetic saturation intensity of cemented carbide is (COML +1.09×COM H ) / 2 when the corresponding carbon content is used for carbon matching;

[0010] When the humidity RH≤55%, the magnetic saturation intensity of cemented carbide is (COM -L +1.05×COM H ) / 2 when the corresponding carbon content is used for carbon blending.

[0011] As a preferred solution of the method for controlling the carbon content of cemented carbide described in the present invention, the cemented carbide is a WC-Co product.

[0012] As a preferred embodiment of the method for controlling the carbon content of cemented carbide described in the present invention, in step S1, the carbon content is increased or decreased by taking the total carbon content of cemented carbide as the center until the carburizing grade C02 and the decarburization grade E02 appear, and the carbon window limit range of the cemented carbide two-phase region is obtained, and the magnetic saturation intensity range COM of the carbon window limit range of the two-phase region is obtained at the same time. L ~COM H .

[0013] As a preferred embodiment of the method for controlling the carbon content of cemented carbide according to the present invention, in step S1, the carbon content increase or decrease is carried out based on the total carbon content of the cemented carbide as the center, specifically:

[0014] When the Co content of cemented carbide is ≤6.0wt.%, the cemented carbide is adjusted by increasing or decreasing the carbon content by 0.015wt.%;

[0015] When 6.0wt.%<the Co content of cemented carbide≤15wt.%, the cemented carbide is adjusted by increasing or decreasing the carbon content by 0.03wt.%;

[0016] When the Co content of cemented carbide is greater than 15wt.%, the carbon content of cemented carbide can be increased or decreased by 0.06wt.% to adjust the materials.

[0017] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0018] A method for preparing cemented carbide comprises the following steps:

[0019] Sa. Using the above control method to achieve carbon matching of cemented carbide;

[0020] Sb. The carbon-matched cemented carbide raw material compact is placed in a plasma sprayed fully coated boat for sintering.

[0021] As a preferred embodiment of the method for preparing cemented carbide according to the present invention, in said step Sb, when the humidity RH>85%, the carbon-matched cemented carbide raw material is sintered within 24 hours after being pressed;

[0022] When the humidity is 55<RH≤85%, the carbon-matched cemented carbide raw material is sintered within 48 hours after being pressed;

[0023] When the humidity RH≤55%, the carbon-matched cemented carbide raw material is sintered within 96 hours after being pressed.

[0024] The beneficial effects of the present invention are as follows:

[0025] The present invention provides a method for controlling the carbon content of cemented carbide and a method for preparing cemented carbide, according to the magnetic saturation intensity range COM of the carbon window limit range of the two-phase region of the qualified cemented carbide product L ~COM H As well as the humidity RH of the production environment, the carbon content of the cemented carbide is controlled, which reduces the probability of the three-phase zone appearing in the product. At the same time, the use of plasma sprayed fully coated boats for sintering will not cause carbon escape, which reduces the interference of the carbon atmosphere during the sintering process, improves the stability of the carbon atmosphere, and further promotes the quality stability of the product in long-term production. DETAILED DESCRIPTION

[0026] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The main purpose of the present invention is to provide a method for controlling the carbon content of cemented carbide and a method for preparing cemented carbide, which can reduce the risk of large-scale decarburization and carburization problems in products and improve the product qualification rate.

[0028] According to one aspect of the present invention, the present invention provides the following technical solution:

[0029] A method for controlling the carbon content of cemented carbide comprises the following steps:

[0030] S1. Determine the magnetic saturation intensity range COM of the carbon window limit range of the cemented carbide two-phase region L ~COM H ;

[0031] S2. Based on the magnetic saturation intensity range COM of step S1 according to different humidity RH L ~COM H Control the carbon content of cemented carbide, specifically:

[0032] When the humidity RH>85%, the magnetic saturation intensity of cemented carbide is (COM L +1.15×COM H ) / 2 when the corresponding carbon content is used for carbon matching;

[0033] When 55<humidity RH≤85%, the magnetic saturation intensity of cemented carbide is (COM L +1.09×COM H ) / 2 when the corresponding carbon content is used for carbon matching;

[0034] When the humidity RH≤55%, the magnetic saturation intensity of cemented carbide is (COM -L +1.05×COM H ) / 2 when the corresponding carbon content is used for carbon blending.

[0035] As a preferred solution of the method for controlling the carbon content of cemented carbide described in the present invention, the cemented carbide is a WC-Co product.

[0036] As a preferred embodiment of the method for controlling the carbon content of cemented carbide described in the present invention, in step S1, the carbon content is increased or decreased by taking the total carbon content of cemented carbide as the center until the carburizing grade C02 and the decarburization grade E02 appear, and the carbon window limit range of the cemented carbide two-phase region is obtained, and the magnetic saturation intensity range COM of the carbon window limit range of the two-phase region is obtained at the same time. L ~COM H .

[0037] As a preferred embodiment of the method for controlling the carbon content of cemented carbide according to the present invention, in step S1, the carbon content increase or decrease is carried out based on the total carbon content of the cemented carbide as the center, specifically:

[0038] When the Co content of cemented carbide is ≤6.0wt.%, the cemented carbide is adjusted by increasing or decreasing the carbon content by 0.015wt.%;

[0039] When 6.0wt.%<the Co content of cemented carbide≤15wt.%, the cemented carbide is adjusted by increasing or decreasing the carbon content by 0.03wt.%;

[0040] When the Co content of cemented carbide is greater than 15wt.%, the carbon content of cemented carbide can be increased or decreased by 0.06wt.% to adjust the materials.

[0041] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0042] A method for preparing cemented carbide comprises the following steps:

[0043] Sa. Using the above control method to achieve carbon matching of cemented carbide;

[0044] Sb. The carbon-matched cemented carbide raw material compact is placed in a plasma sprayed fully coated boat for sintering.

[0045] As a preferred embodiment of the method for preparing cemented carbide according to the present invention, in said step Sb, when the humidity RH>85%, the carbon-matched cemented carbide raw material is sintered within 24 hours after being pressed;

[0046] When the humidity is 55<RH≤85%, the carbon-matched cemented carbide raw material is sintered within 48 hours after being pressed;

[0047] When the humidity RH≤55%, the carbon-matched cemented carbide raw material is sintered within 96 hours after being pressed.

[0048] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0049] Example 1

[0050] A method for preparing cemented carbide comprises the following steps:

[0051] Sa. Carbide with carbon;

[0052] S1. Carbon window analysis of WC-6Co products: With the total carbon of production control as the center, the ingredients are increased or decreased by 0.015wt.% until C02 (carburizing grade) and E02 (decarburization grade) appear and then stop, confirm the carbon window limit range of the two-phase region of WC-6Co products, and obtain the magnetic saturation intensity range of the carbon window limit range of the two-phase region as 3.94-5.41;

[0053] S2. The humidity RH during production is 90%, and the magnetic saturation intensity of cemented carbide is (COM L +1.15×COM H ) / 2=(3.94+1.15×5.41) / 2=5.08, and the corresponding carbon content is 5.82wt.% for carbon blending;

[0054] Sb. After the carbon-matched cemented carbide raw material was pressed into a plasma sprayed fully coated boat for 12 hours, ten batches of sintering were carried out. No decarburization or carburization occurred in the cemented carbide products.

[0055] Example 2

[0056] The difference from Example 1 is that

[0057] S2. The humidity RH during production is 79%, and the magnetic saturation intensity of cemented carbide is (COM L +1.09×COM H) / 2=(3.94+1.09×5.41) / 2=4.92, corresponding to a carbon content of 5.81wt.% for carbon blending;

[0058] Sb. After the carbon-matched cemented carbide raw material was pressed, it was placed in a plasma sprayed fully coated boat for 24 hours and sintered in ten batches. No decarburization or carburization occurred in the cemented carbide products.

[0059] Example 3

[0060] The difference from Example 1 is that

[0061] S2. The humidity RH during production is 50%, and the magnetic saturation intensity of cemented carbide is (COM L +1.05×COM H ) / 2=(3.94+1.05×5.41) / 2=4.81, corresponding to a carbon content of 5.80wt.% for carbon blending;

[0062] Sb. After the carbon-matched cemented carbide raw material was pressed, it was placed in a plasma sprayed fully coated boat for 24 hours and sintered in ten batches. No decarburization or carburization occurred in the cemented carbide products.

[0063] Example 4

[0064] A method for preparing cemented carbide comprises the following steps:

[0065] Sa. Carbide with carbon;

[0066] S1. Carbon window analysis of WC-10Co products: With the total carbon of production control as the center, the ingredients are increased or decreased by 0.03wt.% until C02 (carburizing grade) and E02 (decarburization grade) appear, and then stop to confirm the carbon window limit range of the two-phase region of WC-10Co products. At the same time, the magnetic saturation intensity range of the carbon window limit range of the two-phase region is obtained to be 6.50-8.76;

[0067] S2. The humidity RH during production is 88%, and the magnetic saturation intensity of cemented carbide is (COM L +1.15×COM H ) / 2=(6.50+1.15×8.76) / 2=8.29, and the corresponding carbon content is 5.47wt.% for carbon blending;

[0068] Sb. After the carbon-matched cemented carbide raw material was pressed into a plasma sprayed fully coated boat for 12 hours, ten batches of sintering were carried out. No decarburization or carburization occurred in the cemented carbide products.

[0069] Example 5

[0070] The difference from Example 4 is that

[0071] S2. The humidity RH during production is 72%, and the magnetic saturation intensity of cemented carbide is (COM L +1.09×COM H ) / 2=(6.50+1.09×8.76) / 2=8.02, and the corresponding carbon content is 5.44wt.% for carbon blending;

[0072] Sb. After the carbon-matched cemented carbide raw material was pressed, it was placed in a plasma sprayed fully coated boat for 24 hours and sintered in ten batches. No decarburization or carburization occurred in the cemented carbide products.

[0073] Example 6

[0074] The difference from Example 4 is that

[0075] S2. The humidity RH during production is 45%, and the magnetic saturation intensity of cemented carbide is (COM L +1.05×COM H ) / 2=(6.50+1.05×8.76) / 2=7.85, corresponding to a carbon content of 5.43wt.% for carbon blending;

[0076] Sb. After the carbon-matched cemented carbide raw material was pressed, it was placed in a plasma sprayed fully coated boat for 24 hours and sintered in ten batches. No decarburization or carburization occurred in the cemented carbide products.

[0077] Example 7

[0078] A method for preparing cemented carbide comprises the following steps:

[0079] Sa. Carbide with carbon;

[0080] S1. Carbon window analysis of WC-25Co products: With the total carbon of production control as the center, the ingredients are increased or decreased by 0.06wt.% until C02 (carburizing grade) and E02 (decarburization grade) appear and then stop, confirm the carbon window limit range of the two-phase region of WC-25Co products, and obtain the magnetic saturation intensity range of the carbon window limit range of the two-phase region as 18.21-23.79;

[0081] S2. The humidity RH during production is 92%, and the magnetic saturation intensity of cemented carbide is (COM L +1.15×COM H ) / 2=(18.21+1.15×23.79) / 2=22.78, and the corresponding carbon content is 4.55wt.% for carbon blending;

[0082] Sb. After the carbon-matched cemented carbide raw material was pressed into a plasma sprayed fully coated boat for 12 hours, ten batches of sintering were carried out. No decarburization or carburization occurred in the cemented carbide products.

[0083] Example 8

[0084] The difference from Example 7 is that

[0085] S2. The humidity RH during production is 63%, and the magnetic saturation intensity of cemented carbide is (COM L +1.09×COM H ) / 2=(18.21+1.09×23.79) / 2=22.07, and the corresponding carbon content is 4.50wt.% for carbon blending;

[0086] Sb. After the carbon-matched cemented carbide raw material was pressed, it was placed in a plasma sprayed fully coated boat for 24 hours and sintered in ten batches. No decarburization or carburization occurred in the cemented carbide products.

[0087] Example 9

[0088] The difference from Example 7 is that

[0089] S2. The humidity RH during production is 47%, and the magnetic saturation intensity of cemented carbide is (COM L +1.05×COM H ) / 2=(18.21+1.05×23.79) / 2=21.59, and the corresponding carbon content is 4.47wt.% for carbon blending;

[0090] Sb. After the carbon-matched cemented carbide raw material was pressed, it was placed in a plasma sprayed fully coated boat for 24 hours and sintered in ten batches. No decarburization or carburization occurred in the cemented carbide products.

[0091] Comparative Example 1

[0092] The difference from Example 4 is that the humidity RH is 90%, the Sa control carbon preparation process is not performed, and the carbon preparation is performed according to the carbon content of 5.44wt.%;

[0093] After the carbon-matched cemented carbide raw material was pressed into a green compact, it was placed in a plasma sprayed fully coated boat for sintering 12 hours later. The cemented carbide product showed E02 decarburization.

[0094] Comparative Example 2

[0095] The difference from Example 4 is that the humidity RH is 95%, the Sa control carbon blending process is not performed, and the carbon blending is performed according to the carbon content of 5.44wt.%;

[0096] After the carbon-matched cemented carbide raw material was pressed into a green compact and placed in a plasma sprayed fully coated boat for sintering 12 hours later, the cemented carbide product showed E02-decarburization phenomenon.

[0097] Comparative Example 3

[0098] The difference from Example 4 is that the humidity RH is 30%, the Sa control carbon preparation process is not performed, and the carbon preparation is performed according to the carbon content of 5.44wt.%;

[0099] After the carbon-matched cemented carbide raw material was pressed into a green compact, it was placed in a plasma sprayed fully coated boat for sintering 24 hours later, and the cemented carbide product showed C02-carburization.

[0100] Comparative Example 4

[0101] The difference from Example 5 is that the conventional carbon-based boat is used for sintering, and CO4 carburization occurs in the cemented carbide product.

[0102] The present invention is based on the magnetic saturation intensity range COM of the carbon window limit range of the two-phase region of the qualified cemented carbide product L ~COM H And the production environment humidity RH, control the carbon content of cemented carbide, reduce the probability of three-phase zone in the product, and at the same time, no carbon escape will occur when sintering is carried out using a plasma sprayed fully coated boat, which reduces the interference of the carbon atmosphere during the sintering process, improves the stability of the carbon atmosphere, and further promotes the quality stability of the product in long-term production. Comparative Examples 1-3 that do not use the carbon content control method described in the present invention and Comparative Example 4 that does not use the plasma sprayed fully coated boat described in the present invention cannot achieve stable control of the quality of the cemented carbide product, which is not conducive to large-scale industrial production.

[0103] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for controlling the carbon content of cemented carbide, characterized in that: The steps include: S1. Determine the magnetic saturation intensity range COM of the carbon window limit range of the cemented carbide two-phase region L ~COM H ; Taking the total carbon content of cemented carbide as the center, the carbon content is increased or decreased until the carburizing grade C02 and the decarburization grade E02 appear, and the carbon window limit range of the cemented carbide two-phase zone is obtained, and the magnetic saturation intensity range COM of the carbon window limit range of the two-phase zone is obtained at the same time L ~COM H ; S2. According to the different production environment humidity RH, based on the magnetic saturation intensity range COM of step S1 L ~COM H Control the carbon content of cemented carbide, specifically: When the humidity RH>85%, the magnetic saturation intensity of cemented carbide is (COM L +1.15×COM H ) / 2 when the corresponding carbon content is used for carbon matching; When 55<humidity RH≤85%, the magnetic saturation intensity of cemented carbide is (COM L +1.09×COM H ) / 2 when the corresponding carbon content is used for carbon matching; When the humidity RH≤55%, the magnetic saturation intensity of cemented carbide is (COM -L +1.05×COM H ) / 2 when the corresponding carbon content is used for carbon blending.

2. The method for controlling the carbon content of cemented carbide according to claim 1, characterized in that: The cemented carbide is a WC-Co product.

3. The method for controlling the carbon content of cemented carbide according to claim 2, characterized in that: In step S1, the carbon content increase or decrease of the cemented carbide is carried out based on the total carbon content of the cemented carbide. Specifically, When the Co content of cemented carbide is ≤6.0wt.%, the cemented carbide is adjusted by increasing or decreasing the carbon content by 0.015wt.%; When 6.0wt.%<the Co content of cemented carbide≤15wt.%, the cemented carbide is adjusted by 0.03wt.% to increase or decrease the carbon content; When the Co content of cemented carbide is greater than 15wt.%, the carbon content of cemented carbide can be increased or decreased by 0.06wt.% to achieve batching.

4. A method for preparing cemented carbide, characterized in that: The steps include: Sa. Carbide carbon matching is achieved by using the cemented carbide carbon matching control method according to any one of claims 1 to 3; Sb. The carbon-matched cemented carbide raw material compact is placed in a plasma sprayed fully coated boat for sintering.

5. The method for preparing cemented carbide according to claim 4, characterized in that: In the step Sb, when the humidity RH>85%, the carbon-matched cemented carbide raw material is sintered within 24 hours after being pressed; When the humidity is 55<RH≤85%, the carbon-matched cemented carbide raw material is sintered within 48 hours after being pressed; When the humidity RH≤55%, the carbon-matched cemented carbide raw material is sintered within 96 hours after being pressed.