A kind of furanyl glycidyl ether and its preparation method and application
By introducing furyl glycidyl ether into epoxy resin to form a crosslinking network, the problem of insufficient mechanical properties and heat resistance of bisphenol A type glycidyl ether is solved, and the mechanical properties and heat resistance of epoxy resin are improved. , suitable for adhesives, electronic printed circuit boards and packaging materials.
Patent Information
- Application Number
- CN202211593093.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-13
AI Technical Summary
The existing bisphenol A type glycidyl ethers have shortcomings in terms of mechanical properties and heat resistance, and their production relies on non-renewable resources, resulting in limited application of epoxy resins.
Furanyl glycidyl ether is prepared by condensation, ring-opening and closed-loop reactions using furfural and eugenol as raw materials, and combined with bisphenol A epoxy resin to form a crosslinking network to improve mechanical properties and heat resistance.
It significantly improves the mechanical properties and heat resistance of epoxy resins, especially impact resistance, extends the curing time and increases the glass transition temperature, and expands the application range of materials.
Smart Images

Figure CN115974859B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic synthesis, and specifically relates to furanyl glycidyl ether and a preparation method and application thereof. Background Art
[0002] Epoxy resin has excellent adhesion, chemical stability and electrical insulation properties, and is widely used in various fields such as adhesives, electronic printed circuit boards and packaging materials. At present, more than 90% of commercial epoxy resins are bisphenol A glycidyl ether. Bisphenol A glycidyl ether has many advantages, such as easy molding, excellent insulation properties and outstanding bonding ability. However, like many general-purpose plastics, bisphenol A glycidyl ether also has some shortcomings, such as poor mechanical properties. In addition, with the increasing depletion of non-renewable resources such as petroleum and the continuous improvement of people's green environmental awareness, how to solve the mechanical properties and poor heat resistance of bisphenol A glycidyl ether through renewable resources is an urgent problem to be solved in this field. Summary of the invention
[0003] The purpose of the present invention is to provide a furanyl glycidyl ether and a preparation method and application thereof. The furanyl glycidyl ether provided by the present invention can improve the mechanical properties and heat resistance of epoxy resin, and uses renewable biomass resources as raw materials, so it has good environmental protection.
[0004] In order to achieve the above object, the present invention provides the following technical solutions:
[0005] The present invention provides a furanyl glycidyl ether, the structural formula of which is shown in Formula I:
[0006]
[0007] The present invention also provides a method for preparing the furanyl glycidyl ether described in the above scheme, comprising the following steps:
[0008] (1) mixing furfural, eugenol, a solvent and a first catalyst for condensation reaction to obtain bishydroxyphenyl furan methane;
[0009] (2) mixing the bishydroxyphenyl furan methane, epichlorohydrin and a phase transfer catalyst to carry out a ring-opening reaction to obtain a chlorohydrin ether;
[0010] (3) mixing the chlorohydrin ether and sodium hydroxide to carry out a ring-closure reaction to obtain furanyl glycidyl ether.
[0011] Preferably, the molar ratio of furfural to eugenol is 1:2-4; the ratio of the mass of the first catalyst to the sum of the mass of furfural and eugenol is 0.1-8:100; the molar ratio of bishydroxyphenylfuran methane to epichlorohydrin is 1:2-10; the ratio of the mass of the phase transfer catalyst to the sum of the mass of bishydroxyphenylfuran methane and epichlorohydrin is 0-1:100; the molar ratio of the chlorohydrin ether to sodium hydroxide is 1:2-6.
[0012] Preferably, the reaction temperature of the condensation reaction is 60-100° C., and the reaction time is 2-10 h.
[0013] Preferably, the reaction temperature of the ring-opening reaction is 20 to 100° C., and the reaction time is 1 to 8 hours.
[0014] Preferably, the reaction temperature of the ring-closing reaction is 20-40° C., and the reaction time is 2-8 h.
[0015] Preferably, the first catalyst includes an acidic catalyst or a basic catalyst; the acidic catalyst includes a protonic acid or a Lewis acid; the basic catalyst includes one or more of alkali metal hydroxides, sodium alcoholates, potassium alcoholates, tertiary amines, imidazole salts, pyridine and basic ionic liquids.
[0016] Preferably, the phase transfer catalyst is a quaternary ammonium salt.
[0017] The present invention also provides the use of the furanyl glycidyl ether described in the above scheme or the furanyl glycidyl ether obtained by the preparation method described in the above scheme in the modification of bisphenol A epoxy resin.
[0018] Preferably, the application comprises the following steps: mixing furanyl glycidyl ether, bisphenol A epoxy resin and a curing agent, and then curing and aging the mixture in sequence to obtain a cured epoxy resin.
[0019] The present invention provides a furanyl glycidyl ether, the structural formula of which is shown in Formula I. The furanyl glycidyl ether provided by the present invention is added to an epoxy resin, the modified epoxy resin increases a rigid group furan ring, and the diepoxy group reacts with a curing agent to polymerize into a cross-linked network, thereby improving the elongation at break and tensile strength of the epoxy resin, thereby significantly improving the mechanical properties and heat resistance of the epoxy resin, and in particular significantly improving the impact resistance of the epoxy resin.
[0020] The present invention also provides a method for preparing the furanyl glycidyl ether described in the above scheme. The preparation method provided by the present invention uses furfural, eugenol, epichlorohydrin and sodium hydroxide as raw materials, first synthesizes monomer bishydroxyphenyl furan methane, and then epoxidizes to prepare furanyl glycidyl ether. The obtained furanyl glycidyl ether is added to bisphenol A epoxy resin, the curing speed is accelerated, the diepoxy group increases the crosslinking density, and the glass transition temperature and heat resistance of the bisphenol A epoxy resin after curing are increased; the aromatic ring is introduced into the bisphenol A epoxy resin molecule, the rigidity of the bisphenol A epoxy resin molecular chain is increased, the internal rotation of the chain segment is difficult, and the glass transition temperature of the bisphenol A epoxy resin is increased. The above two factors work together to significantly improve the heat resistance of the bisphenol A epoxy resin. The present invention uses furfural and eugenol as raw materials, and the raw materials used are renewable bio-based monomers, which conforms to the sustainable principle of sustainable development.
[0021] The present invention also provides the use of the furanyl glycidyl ether described in the above scheme or the furanyl glycidyl ether obtained by the preparation method described in the above scheme in the modification of bisphenol A epoxy resin. The furanyl glycidyl ether provided by the present invention is used for epoxy resin modification, which can significantly improve the mechanical properties and heat resistance of materials such as epoxy resin, expand the applicable scope of the material, and the obtained epoxy resin cured product can be used for adhesives, electronic printed circuit boards or packaging materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0023] Figure 1 The infrared spectra of bishydroxyphenyl furan methane (a) prepared in Example 1 of the present invention and furanyl glycidyl ether (b) prepared in Example 6;
[0024] Figure 2 The bishydroxyphenyl furan methane (a) prepared in Example 1 of the present invention and the furanyl glycidyl ether (b) prepared in Example 6 are 13 CNMR (600MHz) images;
[0025] Figure 3 DSC graphs of the epoxy resin cured product (a) prepared in Application Example 1 of the present invention and the epoxy resin cured product (b) prepared in Application Example 3;
[0026] Figure 4 The thermogravimetric curve (A) and thermogravimetric differential curve (B) of the epoxy resin cured products prepared in Application Examples 1 and 3 of the present invention. DETAILED DESCRIPTION
[0027] The present invention provides a furanyl glycidyl ether, the structural formula of which is shown in Formula I:
[0028]
[0029] The present invention also provides a method for preparing the furanyl glycidyl ether described in the above scheme, comprising the following steps:
[0030] (1) mixing furfural, eugenol, a solvent and a first catalyst for condensation reaction to obtain bishydroxyphenyl furan methane;
[0031] (2) mixing the bishydroxyphenyl furan methane, epichlorohydrin and a phase transfer catalyst to carry out a ring-opening reaction to obtain a chlorohydrin ether;
[0032] (3) mixing the chlorohydrin ether and sodium hydroxide to carry out a ring-closure reaction to obtain furanyl glycidyl ether.
[0033] In the present invention, furfural, eugenol, a solvent and a first catalyst are mixed for condensation reaction to obtain bishydroxyphenyl furan methane. In the present invention, the solvent preferably includes one or more of alcohol, amine, benzene homologue and water; the alcohol preferably includes one or more of methanol, ethanol and isopropanol; the amine is preferably triethylamine; the benzene homologue preferably includes one or two of toluene and xylene; the water is preferably deionized water; the first catalyst preferably includes an acidic catalyst or a basic catalyst, more preferably a basic catalyst; the acidic catalyst preferably includes a protonic acid or a Lewis acid; the protonic acid preferably includes one or both of sulfuric acid and phosphoric acid; the Lewis acid preferably includes one or more of TiCl4, InCl3 and SnCl2; the basic catalyst preferably includes an alkali metal hydrogen One or more of oxides, sodium alcoholates, potassium alcoholates, tertiary amines, imidazole salts, pyridine and alkaline ionic liquids; the alkali metal hydroxide preferably includes one or both of sodium hydroxide and potassium hydroxide; the sodium alcoholate preferably includes one or both of sodium methoxide and sodium ethoxide; the potassium alcoholate preferably includes one or more of potassium ethoxide and potassium butoxide; the tertiary amine preferably includes one or both of triethylamine and N,N-dimethyl-n-octylamine; the imidazole salt preferably includes one or both of 1-methylimidazolium chloride and 1-butyl-3-methylimidazolium chloride; the alkaline ionic liquid preferably includes one or both of 1-butyl-3-methylimidazolium hydroxide and 1-butyl-3-methylimidazolium acetate.
[0034] In the present invention, the molar ratio of furfural and eugenol is preferably 1:2-4, more preferably 1:2.5-3.5, and further preferably 1:3; the ratio of the mass of the first catalyst to the sum of the mass of furfural and eugenol is preferably 0.1-8:100, more preferably 0.5-7:100, and further preferably 2-5:100; the ratio of the mass of the solvent to the sum of the mass of furfural and eugenol is preferably 5-60:100, and more preferably 10-50:100; the reaction temperature of the condensation reaction is preferably 60-100°C, more preferably 70-90°C, and the reaction time is preferably 2-10h, and more preferably 4-7h; the condensation reaction is preferably carried out under protective gas conditions; the protective gas is preferably an inert gas; the inert gas is preferably N2. In a specific embodiment of the present invention, eugenol and a solvent are preferably added to a four-necked flask equipped with a mechanical stirrer with a mechanical seal, a reflux condenser and a thermometer at room temperature, N2 is introduced, and then the temperature is raised to the reaction temperature of the condensation reaction, and furfural is then added dropwise; the condensation reaction time is counted from the end of the furfural addition.
[0035] In the present invention, after the condensation reaction is completed, post-treatment is preferably performed; the post-treatment is preferably to cool, neutralize and distill the reaction solution obtained by the condensation reaction in sequence, and then take out the mixture and filter, wash, recrystallize and dry in sequence to obtain bishydroxyphenyl furan methane. In the present invention, the final temperature of the cooling is preferably 10-40°C, more preferably 30°C; the neutralization is preferably to adjust the pH of the reaction solution to 6-7, more preferably 7; the neutralization reagent is preferably acetic acid; the present invention has no special requirements for the distillation, and the solvent can be removed by conventional distillation operation; the present invention has no special requirements for the filtration, and conventional filtration operation can be used; the washing reagent is preferably water; the water is preferably deionized water; the recrystallization is preferably to add the filter cake obtained by filtration and washing to toluene for recrystallization; the drying method is preferably drying; the present invention has no special requirements for the drying, and conventional drying operation can be used.
[0036] In a specific embodiment of the present invention, the industrial sources of furfural include corn cobs, bagasse, cottonseed hulls and rice husks. These crop residues contain polypentose, which can be hydrolyzed in an acidic medium to generate furfural. The molecular structure of furfural contains functional groups such as carbonyl, diene and cyclic ether, so it has the properties of compounds such as aldehydes, ethers, dienes and aromatic hydrocarbons. Eugenol exists in extracts of various plants, and its content is highest in clove oil and bay leaf oil. Eugenol has multiple easily reactive sites (hydroxyl, double bond and benzene ring), thereby generating various resin monomers such as epoxy, acrylic acid and benzoxazine.
[0037] After obtaining bishydroxyphenyl furan methane, the present invention mixes the bishydroxyphenyl furan methane, epichlorohydrin and a phase transfer catalyst to perform a ring-opening reaction to obtain chlorohydrin ether. In the present invention, the phase transfer catalyst is preferably a quaternary ammonium salt; the quaternary ammonium salt preferably includes one or more of benzyltriethylammonium chloride, benzyltrimethylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium chloride, tetrabutylammonium hydrogen sulfate, trioctylmethylammonium chloride, dodecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride and hexadecyltrimethylammonium chloride, dodecyldimethyl dipolyglycerol ether ammonium chloride; the molar ratio of the bishydroxyphenyl furan methane to epichlorohydrin is preferably 1:2 to 10, more preferably The ratio of the mass of the phase transfer catalyst to the mass of bishydroxyphenyl furan methane and epichlorohydrin is preferably 0 to 1:100, more preferably 0.1 to 0.9:100, and more preferably 0.4 to 0.7:100; the reaction temperature of the ring-opening reaction is preferably 20 to 100°C, more preferably 40 to 80°C, and the reaction time is preferably 1 to 8h, more preferably 3 to 6h; the ring-opening reaction is preferably carried out under N2 protection. In a specific embodiment of the present invention, bishydroxyphenyl furan methane and a phase transfer catalyst are preferably added to a four-necked flask equipped with a mechanical stirrer with a mechanical seal, a reflux condenser and a thermometer at room temperature, N2 is introduced, and then the temperature is raised to the reaction temperature of the ring-opening reaction, and then epichlorohydrin is added dropwise for ring-opening reaction, and the time of the ring-opening reaction is counted from the end of the dropwise addition of epichlorohydrin.
[0038] After obtaining the chlorohydrin ether, the present invention mixes the chlorohydrin ether and sodium hydroxide for a ring-closure reaction to obtain furanyl glycidyl ether. In the present invention, the sodium hydroxide is preferably used in the form of solid sodium hydroxide or sodium hydroxide solution, more preferably sodium hydroxide solution, and the concentration of the sodium hydroxide solution is preferably 18-48wt%, more preferably 32wt%; the molar ratio of the chlorohydrin ether to sodium hydroxide is preferably 1:2-6, more preferably 1:3-5, more preferably 1:3.5-4.5; in a specific embodiment of the present invention, after the ring-opening reaction is completed, the obtained reaction solution does not need to be post-treated, and the reaction solution is directly cooled to the temperature of the ring-closure reaction, and then sodium hydroxide is added to carry out the ring-closure reaction.
[0039] In the present invention, the reaction temperature of the ring-closing reaction is preferably 20 to 40° C., more preferably 25 to 35° C., and the reaction time is preferably 2 to 8 h, more preferably 4 to 6 h.
[0040] In the present invention, after the ring-closing reaction is completed, post-treatment is preferably performed; the post-treatment is preferably filtering, washing and distilling the reaction solution obtained by the ring-closing reaction in sequence; the present invention has no special requirements for the filtration, and the filtration operation commonly used in the art can be used; the washing reagent is preferably water, and the water is preferably deionized water; the distillation is preferably reduced pressure distillation, and the excess epichlorohydrin is removed by reduced pressure distillation and recycled.
[0041] The present invention also provides the use of the furanyl glycidyl ether described in the above scheme or the furanyl glycidyl ether obtained by the preparation method described in the above scheme in the modification of bisphenol A epoxy resin.
[0042] In the present invention, the application preferably includes the following steps: mixing furanyl glycidyl ether, bisphenol A epoxy resin and curing agent, and then curing and aging in sequence to obtain epoxy resin cured product. In the present invention, the bisphenol A epoxy resin is preferably E-51 epoxy resin; the curing agent is preferably 4-methyl-hexahydrophthalic anhydride; the mass ratio of furanyl glycidyl ether and bisphenol A epoxy resin is preferably determined according to the purpose of the epoxy resin cured product; the mass of the curing agent is preferably determined according to the epoxy value of the epoxy resin; the mixing method is preferably stirring, and the present invention has no special requirements for the stirring, and the raw materials can be mixed evenly; the curing time and temperature are preferably determined according to the curing kinetics of the resin and the curing agent; the present invention has no special requirements for the aging, and the aging operation commonly used in the art can be used.
[0043] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.
[0044] The raw materials eugenol and furfural used in the present invention are of reagent grade and purchased from Shanghai MacLean Biochemical Technology Co., Ltd.; epichlorohydrin and sodium hydroxide are of industrial grade and purchased from Anhui Xinyuan Technology Co., Ltd.
[0045] The epoxy value of the furanyl glycidyl ether product of the present invention is tested by a hydrochloric acid-acetone method.
[0046] Example 1
[0047] Add 165 g of eugenol, 64 g of ethanol and 2.1 g of triethylamine into a four-necked flask equipped with a mechanical stirrer with a mechanical seal, a reflux condenser and a thermometer, introduce N2, raise the temperature to 60°C, add 48 g of furfural dropwise within 1 hour, react for 4 hours, and cool to 30°C; neutralize with acetic acid to neutrality, and distill out the solvent ethanol; take out the mixture in the flask, filter, and wash with hot water 3 times; take out the filter cake, recrystallize it with toluene 3 times, and dry it to obtain monomer bishydroxyphenylfuranmethane, weighing 19 g.
[0048] Example 2
[0049] Add 246 g of eugenol, 59 g of isopropanol and 5.9 g of sodium hydroxide into a four-necked flask equipped with a mechanical stirrer with a mechanical seal, a reflux condenser and a thermometer, introduce N2, raise the temperature to 85°C, add 48 g of furfural dropwise within 1 hour, react for 6 hours, and cool to 30°C; neutralize with acetic acid to neutrality, and distill out the solvent ethanol; take out the mixture in the flask, filter, and wash with hot water 3 times; take out the filter cake, recrystallize it with toluene 3 times, and dry it to obtain monomer bishydroxyphenylfuranmethane, weighing 42 g.
[0050] Example 3
[0051] Add 328 g of eugenol, 150 g of xylene and 3 g of 1-methylimidazole into a four-necked flask equipped with a mechanical stirrer with a mechanical seal, a reflux condenser and a thermometer, introduce N2, raise the temperature to 100°C, add 48 g of furfural dropwise within 1 hour, react for 9 hours, and cool to 30°C; neutralize with acetic acid to neutrality, and distill out the solvent ethanol; take out the mixture in the flask, filter, and wash with hot water 3 times; take out the filter cake, recrystallize it with toluene 3 times, and dry it to obtain monomer bishydroxyphenylfuranmethane, weighing 80 g.
[0052] Example 4
[0053] 203 g of the monomer bishydroxyphenyl furan methane prepared according to Example 3 and 0.7 g of hexadecyltrimethylammonium chloride were added to a four-necked flask equipped with a mechanical stirrer with a mechanical seal, a reflux condenser and a thermometer, N2 was introduced, the temperature was raised to 40°C, 93 g of epichlorohydrin was added dropwise within 1 hour, and the reaction was kept warm for 4 hours; the temperature was lowered to 30°C, 40 g of solid sodium hydroxide was added in batches within 2 hours, and the reaction was carried out for 4 hours; the obtained reaction liquid was filtered and washed, and the excess epichlorohydrin was distilled under reduced pressure and recovered to obtain 246 g of furanyl glycidyl ether with an epoxide value of 0.2005 mol / 100g.
[0054] Example 5
[0055] 203 g of the monomer bishydroxyphenyl furan methane prepared according to Example 3 and 3.9 g of tetrabutylammonium bromide were added to a four-necked flask equipped with a mechanical stirrer with a mechanical seal, a reflux condenser and a thermometer, N2 was introduced, the temperature was raised to 30°C, 185 g of epichlorohydrin was added dropwise within 1 hour, and then 167 g of 48% sodium hydroxide solution was added dropwise within 1 hour, and the reaction was carried out for 2 hours; the obtained reaction liquid was filtered and washed, and the excess epichlorohydrin was distilled under reduced pressure and recovered to obtain 238 g of furanyl glycidyl ether with an epoxide value of 0.2314 mol / 100g.
[0056] Example 6
[0057] 203 g of the monomer bishydroxyphenyl furan methane prepared according to Example 3 and 4.3 g of dodecyltrimethylammonium chloride were added to a four-necked flask equipped with a mechanical stirrer with a mechanical seal, a reflux condenser and a thermometer, N2 was introduced, the temperature was raised to 80°C, 278 g of epichlorohydrin was added dropwise within 1 hour, and the reaction was kept warm for 2 hours; the temperature was lowered to 40°C, 375 g of 32% sodium hydroxide solution was added dropwise within 1 hour, and the reaction was carried out for 4 hours; the obtained reaction liquid was filtered and washed, and the excess epichlorohydrin was distilled under reduced pressure and recovered to obtain 225 g of furanyl glycidyl ether with an epoxide value of 0.3241 mol / 100g.
[0058] Example 7
[0059] 203 g of the monomer bishydroxyphenyl furan methane prepared according to Example 1 and 5.5 g of dodecyl dimethyl dipolyglycerol ether ammonium chloride were added to a four-necked flask equipped with a mechanical stirrer with a mechanical seal, a reflux condenser and a thermometer, N2 was introduced, the temperature was raised to 90°C, 370 g of epichlorohydrin was added dropwise within 1 hour, and the reaction was kept warm for 1 hour; the temperature was lowered to 20°C, 375 g of 32% sodium hydroxide solution was added dropwise within 1 hour, and the reaction was carried out for 2 hours; the obtained reaction liquid was filtered and washed, and the excess epichlorohydrin was distilled under reduced pressure and recovered to obtain 233 g of furanyl glycidyl ether with an epoxide value of 0.2547 mol / 100g.
[0060] Application Example 1
[0061] Take 45g of E-51 epoxy resin, add 41g of 4-methyl-hexahydrophthalic anhydride curing agent, then add 0.4g of curing accelerator 2-methylimidazole, stir evenly, cure at 90°C for 2h, cure at 120°C for 2h, cure at 160°C for 2h, age at room temperature for 7 days to obtain epoxy resin cured product.
[0062] Application Example 2
[0063] 2 g of furanyl glycidyl ether prepared according to Example 6 was added to 40 g of E-51 epoxy resin, and then 37 g of 4-methyl-hexahydrophthalic anhydride curing agent and 0.4 g of curing accelerator 2-methylimidazole were added. After stirring evenly, the mixture was cured at 90°C for 2 h, at 120°C for 2 h, and at 160°C for 2 h. The mixture was aged at room temperature for 7 days to obtain a cured epoxy resin.
[0064] Application Example 3
[0065] 4 g of furanyl glycidyl ether prepared according to Example 6 was added to 40 g of E-51 epoxy resin, and then 38 g of 4-methyl-hexahydrophthalic anhydride curing agent and 0.4 g of curing accelerator 2-methylimidazole were added. After stirring evenly, the mixture was cured at 90°C for 2 h, 120°C for 2 h, and 160°C for 2 h. The mixture was aged at room temperature for 7 days to obtain a cured epoxy resin.
[0066] Application Example 4
[0067] 6 g of furanyl glycidyl ether prepared according to Example 6 was added to 40 g of E-51 epoxy resin, and then 39 g of 4-methyl-hexahydrophthalic anhydride curing agent and 0.4 g of curing accelerator 2-methylimidazole were added. After stirring evenly, the mixture was cured at 90°C for 2 h, 120°C for 2 h, and 160°C for 2 h, and aged at room temperature for 7 days to obtain a cured epoxy resin.
[0068] Application Example 5
[0069] 8 g of furanyl glycidyl ether prepared according to Example 6 was added to 40 g of E-51 epoxy resin, and then 40 g of 4-methyl-hexahydrophthalic anhydride curing agent and 0.4 g of curing accelerator 2-methylimidazole were added. After stirring evenly, the mixture was cured at 90°C for 2 h, at 120°C for 2 h, and at 160°C for 2 h. The mixture was aged at room temperature for 7 days to obtain an epoxy resin cured product.
[0070] The curing performance of the epoxy resin cured products prepared in Application Examples 1 to 5 of the present invention was tested, and the results are shown in Table 1.
[0071] Table 1 Mechanical properties of epoxy resin cured products prepared in Application Examples 1 to 5 of the present invention
[0072]
[0073]
[0074] It can be seen from Table 1 that the furanyl glycidyl ether provided by the present invention can significantly improve the impact resistance of epoxy resin, and the bending strength is also improved to a certain extent, while the tensile strength does not show a significant decrease, and has good comprehensive mechanical properties.
[0075] The infrared spectrum of the bishydroxyphenyl furan methane prepared in Example 1 and the furanyl glycidyl ether prepared in Example 6 was tested. The results are as follows: Figure 1 As shown. Figure 1 From (a), we can see that 1594cm -1 Characteristic peak of benzene ring, 1493cm -1 It is the characteristic peak of furan ring, 1218cm -1The peak of the asymmetric stretching vibration of the furan ring COC is 1077 cm -1 The peak of furan ring COC symmetric stretching vibration is 3496 cm -1 and 3411cm -1 The stretching vibration of -OH is different, which is caused by the asymmetry of the furan group in the monomer, resulting in the relative difference in the spatial position of the two hydroxyl groups. It can be seen that the present invention successfully prepares the bishydroxyphenyl furan methane monomer; according to Figure 1 From (b), we can see that 1594cm -1 Characteristic peak of benzene ring, 1493cm -1 It is the characteristic peak of furan ring, 1218cm -1 The peak of the asymmetric stretching vibration of the furan ring COC is 1077 cm -1 The peak of furan ring COC symmetric stretching vibration is 911 cm -1 is the characteristic peak of the epoxy group, which shows that the present invention successfully prepares furanyl glycidyl ether.
[0076] The bishydroxyphenyl furan methane prepared in Example 1 of the present invention and the furanyl glycidyl ether prepared in Example 6 were subjected to nuclear magnetic resonance analysis. The results are as follows: Figure 2 As shown. Figure 2 As shown in (a), the deuterated reagent used is d-DMSO, and the chemical shift δ=141.81 ppm is the carbon signal peak connected to the benzene ring and the hydroxyl group. It can be seen that the present invention successfully prepares the bishydroxyphenyl furan methane monomer; according to Figure 2 As shown in (b), the deuterated reagent used is d-CDCl3, and the chemical shifts δ=44.92ppm and δ=50.43ppm are the absorption peaks of the epoxy group, which shows that the present invention successfully prepares furanyl glycidyl ether.
[0077] The gelling property of furanyl glycidyl ether prepared in Example 6 of the present invention was tested. The testing method was as follows: according to the preparation methods of Application Examples 1 to 5, furanyl glycidyl ether prepared in Example 6 of the present invention was added to E-51 resin in amounts of 0, 5 wt%, 10 wt%, 15 wt% and 20 wt% of the E-51 resin, respectively. Then, 4-methyl-hexahydrophthalic anhydride curing agent was added without adding a curing accelerator. The gelling time was tested at 120° C. The results are shown in Table 2.
[0078] Table 2 Gel time of epoxy resin cured product prepared by furanyl glycidyl ether of Example 6
[0079] Addition amount / wt% 0 5 10 15 20 Curing time / min 95 75 43 32 20
[0080] According to Table 2, after the furanyl glycidyl ether prepared by the present invention is added, the gel time of the epoxy resin is greatly reduced and the curing speed is accelerated. It can be seen that the diepoxy group increases the crosslinking density.
[0081] The epoxy resin cured product prepared in Application Example 1 of the present invention and the epoxy resin cured product prepared in Application Example 3 were subjected to differential scanning calorimetry analysis. The results are as follows: Figure 3 As shown. Figure 3 Figure a in the middle is the epoxy resin cured product prepared in Application Example 1. Figure 3 Figure b in the middle is the epoxy resin cured product prepared in Application Example 3. Figure 3 It can be seen that, compared with the epoxy resin cured product prepared in Application Example 1, the epoxy resin cured product incorporating the furanyl glycidyl ether of the present invention has a glass transition temperature increased by 6°C.
[0082] The epoxy resin cured products prepared in Application Examples 1 and 3 of the present invention were tested for thermal stability in a N2 atmosphere. The results are shown in Tables 3 and Figure 4 As shown, Figure 4 Curve a in FIG. 1 represents the sample of the epoxy resin cured material prepared in Application Example 1, and curve b represents the sample of the epoxy resin cured material prepared in Application Example 3.
[0083] Table 3 Thermogravimetric data of epoxy resin cured products prepared in Application Examples 1 and 3 of the present invention
[0084] Application Examples <![CDATA[T 5% (℃)]]> <![CDATA[T 10% (℃)]]> <![CDATA[T 50% (℃)]]> <![CDATA[T max (℃)]]> 1 345.2 368.0 409.7 413.5 3 367.7 383.2 416.4 418.3
[0085] According to Table 3 and Figure 4 It can be seen that compared with Application Example 1, the initial pyrolysis temperature (T i ) is about 22°C higher, which shows that the furanyl glycidyl ether provided by the present invention can improve the heat resistance of epoxy resin.
[0086] It can be seen from the above examples that the furanyl glycidyl ether provided by the present invention can significantly improve the mechanical properties and heat resistance of epoxy resin, especially can significantly improve the impact resistance of epoxy resin, wherein the flexural strength can reach 77.0MPa, and the impact strength can reach 15.8KJ / m 2 , the tensile strength can reach 37.0MPa, and it has good comprehensive mechanical properties.
[0087] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A furanyl glycidyl ether, characterized in that: The structural formula is shown in Formula I: Formula I.
2. The method for preparing furanyl glycidyl ether according to claim 1, comprising the following steps: (1) mixing furfural, eugenol, a solvent and a first catalyst for condensation reaction to obtain a compound represented by formula II; Formula II; (2) mixing the compound represented by formula II, epichlorohydrin and a phase transfer catalyst to carry out a ring-opening reaction to obtain a compound represented by formula III; Formula III; (3) The compound represented by formula III is mixed with sodium hydroxide to carry out a ring-closing reaction to obtain furanyl glycidyl ether, the structure of which is shown in formula I.
3. The preparation method according to claim 2, characterized in that: The molar ratio of furfural to eugenol is 1:2-4; the ratio of the mass of the first catalyst to the sum of the mass of furfural and eugenol is 0.1-8:100; the molar ratio of the compound represented by formula II to epichlorohydrin is 1:2-10; the ratio of the mass of the phase transfer catalyst to the sum of the mass of the compound represented by formula II and epichlorohydrin is 0-1:100; the molar ratio of the compound represented by formula III to sodium hydroxide is 1:2-6.
4. The preparation method according to claim 2 or 3, characterized in that: The reaction temperature of the condensation reaction is 60-100°C, and the reaction time is 2-10 h.
5. The preparation method according to claim 2 or 3, characterized in that: The reaction temperature of the ring-opening reaction is 20-100°C, and the reaction time is 1-8 h.
6. The preparation method according to claim 2 or 3, characterized in that: The reaction temperature of the ring-closing reaction is 20-40° C., and the reaction time is 2-8 h.
7. The preparation method according to claim 2 or 3, characterized in that: The first catalyst is an acidic catalyst or a basic catalyst; The acidic catalyst is a protonic acid or a Lewis acid; The alkaline catalyst is one or more of alkali metal hydroxide, sodium alcoholate, potassium alcoholate, tertiary amine, imidazole salt, pyridine and alkaline ionic liquid.
8. The preparation method according to claim 2 or 3, characterized in that: The phase transfer catalyst is a quaternary ammonium salt.
9. Use of the furanyl glycidyl ether according to claim 1 or the furanyl glycidyl ether obtained by the preparation method according to any one of claims 2 to 8 in the modification of bisphenol A epoxy resin.
10. The use according to claim 9, characterized in that: The application comprises the following steps: mixing furanyl glycidyl ether, bisphenol A epoxy resin and a curing agent, and then sequentially curing and aging to obtain an epoxy resin cured product.
Citation Information
Patent Citations
Biomass-based epoxy resin and preparation method thereof
CN106589317A
Honokiol / glycosyl furan double-bio-based epoxy resin monomer as well as preparation method and application thereof
CN114315814A
Full-bio-based cyano epoxy resin and green preparation method thereof
CN114395110A
Improvements in and relating to Light-Sensitive Reproduction Material
GB1164024A
Phenolic resin, epoxy resin, epoxy resin composition, and cured product of the same
JP2008195843A